Tetraphosphine ligand complex as well as preparation method and application thereof
Through the simplified tetraphosphine ligand complex synthesis method and combination with rhodium precursor, the problems of complexity and low catalytic efficiency of traditional phosphine ligand synthesis are solved, and the efficient olefin hydroformylation reaction is achieved, which improves the catalyst Stability and reaction yield.
Patent Information
- Application Number
- CN202411250119.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The traditional phosphine ligand synthesis method is complex, difficult to operate and low yield, which affects the catalytic efficiency of phosphine ligands in catalytic olefin hydroformylation reaction.
Using tetraphosphine ligand complex and its preparation method, stable tetraphosphine is obtained by reacting phosphine-containing monoamine, 2,6-pyridine diformaldehyde and inorganic salts at a specific molar ratio, combined with inert gas replacement and organic solvent stirring. Ligand complexes and combined with rhodium precursors are used as catalysts for olefin hydroformylation reactions.
The synthesis steps of tetraphosphine ligand are simplified, the operation difficulty is reduced, the stability and catalytic activity of the catalyst are improved, and the selectivity and yield of the olefin hydroformylation reaction are enhanced.
Smart Images

Figure BDA0005032013630000021 
Figure BDA0005032013630000022 
Figure BDA0005032013630000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic synthesis, and in particular relates to a tetraphosphine ligand complex and a preparation method and application thereof. Background Art
[0002] The olefin hydroformylation reaction catalyzed by transition metal complexes is an important method for producing aldehydes from olefins and synthesis gas in industry. With an annual aldehyde production of more than 10 million tons, it has become one of the most important industrial catalytic processes. Aldehydes can be used as pesticides, disinfectants, and preservatives, and are widely used in the fields of medicine, agriculture, and chemical production. Aldehydes can be further converted into amines, alcohols, carboxylic acids, esters, amides, etc., and are important intermediates for the synthesis of softeners, surfactants, and drugs, etc., and have great economic value.
[0003] Phosphine ligand-modified rhodium catalysts have good catalytic activity and selectivity in hydroformylation reactions. However, in traditional phosphine ligand synthesis methods, there are usually problems such as numerous synthesis steps, complex operations, and harsh reaction conditions, which make the synthesis of phosphine ligands, especially polyphosphine ligands, difficult, low in yield, and expensive, which affects the application of phosphine ligands. Therefore, it is very important to develop a green and efficient method for synthesizing polyphosphine ligands.
[0004] With the development of supramolecular self-assembly, strategies for assembling monophosphine ligands into diphosphine ligands have been gradually reported. This strategy requires the rational design of the assembly building blocks of the ligands, and each building block can quickly construct ligands with diverse structures through non-covalent bond forces such as hydrogen bonding, electrostatics, and metal-ligand coordination. The biggest advantage of this strategy is that phosphine ligands can be prepared efficiently and modularly, which to a certain extent overcomes the complex shortcomings of traditional covalent bond phosphine ligand synthesis methods and can exponentially expand the ligand library in a short time. Summary of the invention
[0005] In view of the above-mentioned prior art, the present invention provides a tetraphosphine ligand complex and a preparation method and application thereof, so as to solve the technical problem that the catalytic efficiency of the existing catalysts is low when catalyzing the hydroformylation of olefins.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is to provide a tetraphosphine ligand complex, the structural formula of the tetraphosphine ligand complex is shown in Formula I:
[0007]
[0008] Wherein, R is aryl, cyclohexyl or pyrrolyl;
[0009] M n+ Fe 2+ 、Zn 2+ or Co 3+ ;
[0010] X - OTf - NTf2 - or BF4 - .
[0011] Based on the above technical solution, the present invention can also be improved as follows.
[0012] Further, R is phenyl; X - NTf2 - .
[0013] Further, the tetraphosphine ligand complex is one of the following compounds:
[0014]
[0015] The present invention also discloses a method for preparing the tetraphosphine ligand complex, which comprises the following steps:
[0016] S1: adding a phosphine-containing monoamine, 2,6-pyridinedicarboxaldehyde and an inorganic salt into a reaction container at a molar ratio of 4:2:1, evacuating the reaction container, and replacing the air in the reaction container with an inert gas; the inorganic salt is an iron salt, a zinc salt or a cobalt salt;
[0017] S2: Add an organic solvent to the reaction vessel, stir and react at 40-80°C for 10-15h, and then cool to room temperature;
[0018] S3: removing the organic solvent, then dissolving the residue in a mixed solution of acetonitrile and diethyl ether, performing recrystallization, collecting the crystals, and obtaining a tetraphosphine ligand complex.
[0019] Furthermore, the phosphine-containing monoamine is 4-(diphenylphosphino)aniline or 3-(diphenylphosphino)aniline; the iron salt is ferrous trifluoromethanesulfonate, bis(trifluoromethanesulfonyl)imide iron or ferrous tetrafluoroborate; the zinc salt is zinc trifluoromethanesulfonate, bis(trifluoromethanesulfonyl)imide zinc or zinc tetrafluoroborate; the cobalt salt is bis(trifluoromethanesulfonyl)imide cobalt; the inert gas is argon or nitrogen; and the organic solvent is at least one of acetonitrile, tetrahydrofuran, toluene, dichloromethane and ethyl acetate.
[0020] Furthermore, the stirring reaction time in S2 is 12 h.
[0021] Further, the mixed solution is prepared by mixing acetonitrile and diethyl ether in a volume ratio of 1:50.
[0022] The invention also discloses a catalyst for olefin hydroformylation reaction, comprising a rhodium precursor and the above-mentioned tetraphosphine ligand complex, wherein the molar ratio of the rhodium precursor to the tetraphosphine ligand complex is 1:2-1:4; the rhodium precursor is [RhCl(CH2=CH2)2]2, RhCl3, [Rh(Cp*)Cl2]2, Rh(cod)2BF4, HRh(CO)(TPP)3, [Rh(cod)Cl]2, Rh(acac)(CH2=CH2)2 or Rh(acac)(CO)2, wherein Cp* is pentamethylcyclopentadiene, cod is 1,4-cyclooctadiene, and acac is acetylacetone.
[0023] The present invention also discloses the use of the catalyst in catalyzing olefin hydroformylation. The olefin hydroformylation reaction comprises the following steps:
[0024] Add olefin, catalyst and organic solvent into a high-pressure reactor, replace the air in the reactor with synthesis gas (CO / H2), then fill the reactor with 1-4MPa synthesis gas, and then react at 50-100°C for 5-12h to obtain; the molar ratio of olefin to rhodium precursor in the catalyst is 500-2000:1; the synthesis gas is mixed by CO and H2 in a volume ratio of 1.0:1-1.1:1.
[0025] Furthermore, the olefin is at least one of a low-carbon terminal olefin, a high-carbon chain internal olefin, a cyclic olefin, styrene, an olefin containing an ether bond or an ester group; and the organic solvent is at least one of anisole, toluene, n-hexane, ethyl ether, tetrahydrofuran, xylene, trimethylbenzene, 1,4-dioxane, dichloromethane, chloroform and acetonitrile.
[0026] The beneficial effects of the present invention are:
[0027] 1. The tetraphosphine ligand complex prepared by the present invention has mild synthesis conditions and simple steps, and does not require the use of dangerous reagents such as n-butyl lithium or Grignard reagent for the traditional synthesis of phosphine ligands, thereby reducing the difficulty of operation.
[0028] 2. The tetraphosphine ligand complex prepared by the present invention has good stability and is not easy to deteriorate. The modified rhodium catalyst has good catalytic activity and selectivity in the olefin hydroformylation reaction.
[0029] 3. Rational modification of the molecular building blocks aldehydes and amines is expected to assemble phosphine ligands with more novel and diverse structures. DETAILED DESCRIPTION
[0030] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0031] Example 1
[0032] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0033]
[0034] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0035] S1: 4 mmol of 4-(diphenylphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of bis(trifluoromethylsulfonyl)imide iron were added to a reaction container, vacuumed, and the air in the reaction container was replaced with nitrogen;
[0036] S2: Add 10 mL of ultra-dry acetonitrile to the reaction vessel, stir and react at 70°C for 12 h, and then cool to room temperature;
[0037] S3: remove acetonitrile by distillation under reduced pressure, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain the tetraphosphine ligand complex L1.
[0038] The results of NMR characterization of L1 are as follows:
[0039] 1 H NMR (400MHz, CD3CN, 25℃) δ8.38-8.33(m,5H),7.47(d,J=5.2Hz,12H),7.23–7.19(m,8H),7.01(t,J=7.2Hz,4H),6.37(d,J=7.9Hz,4H)ppm.
[0040] 31 P NMR(162MHz,CD3CN)δ-6.14ppm.
[0041] 13 C NMR (200MHz, CD3CN, 25℃) δ172.2,160.3,147.9,141.0,138.1,137.0,135.1,134.6,130.5,130.4,129.9,121.8ppm.
[0042] Example 2
[0043] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0044]
[0045] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0046] S1: 4 mmol of 3-(diphenylphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of bis(trifluoromethylsulfonyl)imide iron were added to a reaction container, vacuumed, and the air in the reaction container was replaced with nitrogen;
[0047] S2: Add 10 mL of ultra-dry acetonitrile to the reaction vessel, stir and react at 70°C for 12 h, and then cool to room temperature;
[0048] S3: remove acetonitrile by distillation under reduced pressure, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain the tetraphosphine ligand complex L2.
[0049] The results of NMR characterization of L2 are as follows:
[0050] 1 H NMR (400MHz, CD3CN, 25℃) δ8.13(s,6H),7.52(s,4H),7.35–7.21(m,27H),7.19(t,J =7.5Hz,5H),7.13-7.10(m,16H),6.16(d,J=6.7Hz,4H),5.60(d,J=5.0Hz,4H)ppm. 31 P NMR (162MHz, CD3CN, 25℃) δ-5.15ppm.
[0051] Example 3
[0052] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0053]
[0054] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0055] S1: 4 mmol of 4-(diphenylphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of zinc bis(trifluoromethylsulfonyl)imide were added to a reaction vessel, vacuumed, and the air in the reaction vessel was replaced with nitrogen;
[0056] S2: Add 10 mL of ultra-dry acetonitrile to the reaction vessel, stir and react at 70°C for 12 h, and then cool to room temperature;
[0057] S3: remove acetonitrile by distillation under reduced pressure, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain the tetraphosphine ligand complex L3.
[0058] The results of NMR characterization of L3 are as follows:
[0059] 31 P NMR (162MHz, CD3CN, 25℃) δ-5.65ppm.
[0060] Example 4
[0061] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0062]
[0063] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0064] S1: 4 mmol of 4-(diphenylphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of bis(trifluoromethylsulfonyl)imide cobalt are added to a reaction container, vacuuming, and replacing the air in the reaction container with nitrogen;
[0065] S2: Add 10 mL of ultra-dry acetonitrile to the reaction vessel, stir and react at 70°C for 10 h, and then cool to room temperature;
[0066] S3: remove acetonitrile by distillation under reduced pressure, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain the tetraphosphine ligand complex L4.
[0067] The results of NMR characterization of L4 are as follows:
[0068] 31 P NMR (162MHz, CD3CN, 25℃) δ-6.15ppm.
[0069] Example 5
[0070] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0071]
[0072] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0073] S1: 4 mmol of 4-(dipyrrolphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of ferrous trifluoromethanesulfonate were added to a reaction vessel, vacuumed, and the air in the reaction vessel was replaced with nitrogen;
[0074] S2: Add 10 mL of dehydrated and deoxygenated ethyl acetate to the reaction vessel, stir and react at 60°C for 10 h, and then cool to room temperature;
[0075] S3: remove ethyl acetate by distillation under reduced pressure, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain tetraphosphine ligand complex L5.
[0076] Example 6
[0077] A tetraphosphine ligand complex, the synthesis reaction formula of which is as follows:
[0078]
[0079] The tetraphosphine ligand complex in this embodiment is prepared by the following steps:
[0080] S1: 4 mmol of 4-(dicyclohexylphosphino)aniline, 2 mmol of 2,6-pyridinedicarboxaldehyde, and 1 mmol of ferrous tetrafluoroborate were added to a reaction container, vacuumed, and the air in the reaction container was replaced with nitrogen;
[0081] S2: Add 10 mL of dehydrated and deoxygenated dichloromethane to the reaction vessel, stir and react at 40°C for 10 h, and then cool to room temperature;
[0082] S3: distill under reduced pressure to remove dichloromethane, then dissolve the residue in a mixed solution of acetonitrile and diethyl ether (volume ratio 1 / 50), perform recrystallization, collect the crystals, and obtain the tetraphosphine ligand complex L6.
[0083] Experimental Example 1
[0084] L1 is used as a ligand to modify the rhodium precursor; the mixture of L1 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0085]
[0086] The specific steps are:
[0087] 0.5 mL 1-hexene, 7.7 mg tetraphosphine ligand complex L1, 1.1 mg Rh(acac)(CO)2 and 3 mL toluene were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 1 MPa of synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was toluene and hydroformylation products. The conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 45%, and the yield of branched-chain aldehydes was 23%.
[0088] Experimental Example 2
[0089] L2 is used as a ligand to modify the rhodium precursor; the mixture of L2 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0090]
[0091] The specific steps are:
[0092] 0.5 mL 2-octene, 15.4 mg tetraphosphine ligand complex L2, 1.1 mg Rh(acac)(CO)2 and 3 mL toluene were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 1 MPa of synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was toluene and hydroformylation products. The conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The aldehyde yield was 49%.
[0093] Experimental Example 3
[0094] L3 is used as a ligand to modify the rhodium precursor; the mixture of L3 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0095]
[0096] The specific steps are:
[0097] 0.5mL 1-decene, 7.7mg tetraphosphine ligand complex L3, 1.1mg Rh(acac)(CO)2 and 3mL toluene were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 1MPa synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1. The reaction was stirred at 90℃ for 5h, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was toluene and hydroformylation products. The conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 43%, and the yield of branched-chain aldehydes was 24%.
[0098] Experimental Example 4
[0099] L4 is used as a ligand to modify the rhodium precursor; the mixture of L4 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0100]
[0101] The specific steps are:
[0102] 0.5 mL C8 mixed olefins, 7.7 mg tetraphosphine ligand complex L4, 1.1 mg Rh(acac)(CO)2 and 3 mL toluene were mixed, and the mixed solution was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 1 MPa of synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and the reaction was cooled to room temperature after the reaction was completed. The solution in the reactor was toluene and hydroformylation products. The conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The aldehyde yield was 31%.
[0103] Experimental Example 5
[0104] L5 is used as a ligand to modify the rhodium precursor; the mixture of L5 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0105]
[0106] The specific steps are:
[0107] 0.6 mL of styrene, 9.2 mg of tetraphosphine ligand complex L5, 1.2 mg of Rh(acac)(CH=CH2)2 and 3 mL of anisole were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 2 MPa of synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and the reaction was cooled to room temperature after the reaction was completed. The solution in the reactor was anisole and hydroformylation product, and the conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 20%, and the yield of branched-chain aldehydes was 48%.
[0108] Experimental Example 6
[0109] L6 is used as a ligand to modify the rhodium precursor; the mixture of L6 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0110]
[0111] The specific steps are:
[0112] 0.5 mL of propenyl phenyl ether, 11.9 mg of tetraphosphine ligand complex L6, 1.7 mg of Rh(cod)2BF4 and 3 mL of toluene were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring. Synthesis gas replaced the air in the reactor, and 2 MPa of synthesis gas was filled in. The synthesis gas was a mixture of CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was toluene and hydroformylation products. The conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 49%, and the yield of branched-chain aldehydes was 32%.
[0113] Experimental Example 7
[0114] L1 is used as a ligand to modify the rhodium precursor; the mixture of L1 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0115]
[0116] The specific steps are:
[0117] 0.5 mL 1-tetradecene, 27.3 mg tetraphosphine ligand complex L1, 3.9 mg HRh(CO)(TPP)3 and 3 mL tetrahydrofuran were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring, and the air in the reactor was replaced by nitrogen, and 3 MPa of synthesis gas was filled in, and the synthesis gas was mixed with CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 6 hours, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was tetrahydrofuran and hydroformylation product, and the conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 46%, and the yield of branched-chain aldehydes was 48%.
[0118] Experimental Example 8
[0119] L1 is used as a ligand to modify the rhodium precursor; the mixture of L1 and the rhodium precursor is used as a catalyst to catalyze the hydroformylation of olefins. The reaction equation is as follows:
[0120]
[0121] The specific steps are:
[0122] 0.5 mL of 10-enoic acid methyl ester, 7.7 mg of tetraphosphine ligand complex L1, 1.1 mg of Rh(acac)(CO)2 and 3 mL of toluene were mixed, and the mixture was placed in a high-pressure reactor with magnetic stirring, and the air in the reactor was replaced by nitrogen, and 2 MPa of synthesis gas was filled in, and the synthesis gas was mixed with CO and H2 in a volume ratio of 1:1; the reaction was stirred at 90°C for 5 hours, and after the reaction was completed, it was cooled to room temperature. The solution in the reactor was toluene and hydroformylation products, and the conversion rate of olefins and the yield of aldehydes were detected by gas chromatography. The yield of straight-chain aldehydes was 47%, and the yield of branched-chain aldehydes was 30%.
[0123] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A tetraphosphine ligand complex, characterized in that: The structural formula of the tetraphosphine ligand complex is shown in Formula I: Wherein, R is aryl, cyclohexyl or pyrrolyl; M n+ Fe 2+ 、Zn 2+ or Co 3+ ; X - OTf - NTf2 - or BF4 - .
2. The tetraphosphine ligand complex according to claim 1, characterized in that: The R is a phenyl group; the X - NTf2 - .
3. The tetraphosphine ligand complex according to claim 2, characterized in that The tetraphosphine ligand complex is one of the following compounds:
4. The method for preparing the tetraphosphine ligand complex according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: adding a phosphine-containing monoamine, 2,6-pyridinedicarboxaldehyde and an inorganic salt into a reaction container at a molar ratio of 4:2:1, evacuating the reaction container, and replacing the air in the reaction container with an inert gas; the inorganic salt is an iron salt, a zinc salt or a cobalt salt; S2: Add an organic solvent to the reaction vessel, stir and react at 40-80°C for 10-15h, and then cool to room temperature; S3: removing the organic solvent, then dissolving the residue in a mixed solution of acetonitrile and diethyl ether, performing recrystallization, collecting the crystals, and obtaining a tetraphosphine ligand complex.
5. The preparation method according to claim 4, characterized in that: The phosphine-containing monoamine is 4-(diphenylphosphino)aniline or 3-(diphenylphosphino)aniline; the iron salt is ferrous trifluoromethanesulfonate, bis(trifluoromethanesulfonyl)imide iron or ferrous tetrafluoroborate; the zinc salt is zinc trifluoromethanesulfonate, bis(trifluoromethanesulfonyl)imide zinc or zinc tetrafluoroborate; the cobalt salt is bis(trifluoromethanesulfonyl)imide cobalt; the inert gas is argon or nitrogen; and the organic solvent is at least one of acetonitrile, tetrahydrofuran, toluene, dichloromethane and ethyl acetate.
6. The preparation method according to claim 4, characterized in that: The stirring reaction time in S2 is 12 h.
7. The preparation method according to claim 4, characterized in that: The volume ratio of acetonitrile to ether in the mixed solution is 1:
50.
8. A catalyst for olefin hydroformylation, characterized in that: The invention comprises a rhodium precursor and the tetraphosphine ligand complex according to any one of claims 1 to 3, wherein the molar ratio of the rhodium precursor to the tetraphosphine ligand complex is 1:2 to 1:4; the rhodium precursor is [RhCl(CH2=CH2)2]2, RhCl3, [Rh(Cp*)Cl2]2, Rh(cod)2BF4, HRh(CO)(TPP)3, [Rh(cod)Cl]2, Rh(acac)(CH2=CH2)2 or Rh(acac)(CO)2, wherein Cp* is pentamethylcyclopentadiene, cod is 1,4-cyclooctadiene, and acac is acetylacetone.
9. Use of the catalyst according to claim 8 in catalyzing olefin hydroformylation, characterized in that: The reaction of olefin hydroformylation comprises the following steps: Add olefin, catalyst and organic solvent into a high-pressure reactor, replace the air in the reactor with synthesis gas, then fill the reactor with 1-4MPa synthesis gas, and then react at 50-100°C for 5-12h to obtain; the molar ratio of the olefin to the rhodium precursor in the catalyst is 500-2000:1; the synthesis gas is a mixture of CO and H2 in a volume ratio of 1.0:1 to 1.1:
1.
10. The use according to claim 9, characterized in that: The olefin is at least one of low-carbon terminal olefins, high-carbon chain internal olefins, cyclic olefins, styrene, and olefins containing ether bonds or ester groups; the organic solvent is at least one of anisole, toluene, n-hexane, ethyl ether, tetrahydrofuran, xylene, trimethylbenzene, 1,4-dioxane, dichloromethane, chloroform and acetonitrile.
Citation Information
Patent Citations
Bimetal coordination polymer as well as preparation method and application thereof
CN116925377A
Organo-phosphine compound and the catalyst system thereby and its application
CN1258676A