Water-based acrylic emulsion for galvanized steel coating and production method of water-based acrylic emulsion
By using a composite copolymerization technology containing amine-based functional monomers and multiple initiators in aqueous acrylic emulsions, the problems of poor adhesion and corrosion resistance of galvanized steel surface coatings are solved, and high adhesion, water resistance and Salt spray resistance improves the corrosion resistance and storage stability of galvanized steel coatings.
Patent Information
- Application Number
- CN202411278576.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
AI Technical Summary
The adhesion, corrosion resistance and storage stability of existing galvanized steel special paints are poor, especially in water-based paints, which leads to poor wet adhesion of the paint film, prone to flash rust and unstable performance.
Combination copolymerization is performed using functional acrylate monomers containing amino groups such as dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide, combining with a variety of initiators such as azodiisoprene and tert-butyl Hydrogen oxide, optimize the ratio of cationic and nonionic emulsifiers, adjust the pH value and add preservatives to form an optimized aqueous acrylic emulsion production method.
It improves the adhesion, water resistance and salt spray resistance of the coating film, enhances the corrosion resistance, meets the high adhesion and corrosion resistance of the galvanized steel surface, and improves storage stability.
Smart Images

Figure BDA0005040953770000061 
Figure BDA0005040953770000071 
Figure BDA0005040953770000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of production of water-based acrylic emulsions, and in particular relates to a water-based acrylic emulsion for galvanized steel coating and a production method thereof. Background Art
[0002] In water-based paints, the base material plays a decisive role in the performance of the paint film. Acrylic resins are widely used as base materials for paints because of their wide sources, moderate cost, quick drying, high hardness and excellent weather resistance.
[0003] Steel plates are corroded to varying degrees due to environmental factors during storage and use, causing serious economic losses and safety hazards. Applying an anti-corrosion layer on the surface of steel to prevent uniform corrosion, uneven corrosion, pitting corrosion, stress corrosion and other metal corrosion phenomena of steel structures is the most common and cost-effective protective measure.
[0004] Galvanizing is an important means of anti-corrosion and anti-rust for steel. Generally, the surface after hot-dip galvanizing has certain anti-rust and anti-corrosion properties, but the galvanized layer is easily damaged and prone to local rust. Therefore, for many users with anti-corrosion and decoration needs, painting the surface of galvanized steel structures is still the main means.
[0005] However, the surface of galvanized steel is very smooth and has poorer adhesion than ordinary carbon steel. Most paints have poor adhesion and are very easy to fall off. Alkyd paint, nitro paint and even some epoxy paints known for their strong adhesion will have insufficient adhesion and fall off in pieces. Especially when applying alkyd paint, the acid and zinc undergo saponification reaction, which not only causes the loss of the galvanized layer, but also causes waste of paint and rework.
[0006] Existing special paints for galvanized steel include epoxy zinc yellow primer and acrylic polyurethane topcoat or fluorocarbon topcoat, epoxy ester zinc yellow primer and epoxy ester topcoat, or epoxy ester zinc yellow primer and alkyd enamel. However, most of these anti-corrosion coatings are oil-based paints. However, as people's environmental awareness increases, water-based anti-corrosion coatings are becoming more and more popular and have become the direction of industry development.
[0007] In water-based anticorrosion coatings, the base material plays a decisive role in the performance of the paint film. Common base materials for water-based anticorrosion coatings are: water-based acrylic emulsion, water-based alkyd resin, water-based epoxy ester-acrylic resin hybrid, two-component water-based polyurethane, and water-based epoxy resin. Among them, water-based acrylic emulsion is the most cost-effective polymer among various water-based coating film-forming materials due to its excellent weather resistance and convenient construction. Ordinary water-based acrylic anti-rust paints generally have good water and salt water resistance, but poor salt spray resistance. At the same time, the wet adhesion of the paint film is poor, which will cause blistering of the paint film and corrosion of the substrate; it is easy to flash rust. Water-based paints introduce water during the construction stage, and the iron substrate comes into contact with water, resulting in flash rust; in order to improve the anti-corrosion performance, some researchers will introduce a large amount of phosphate esters and silicone monomers into the emulsion, but silicone monomers are easily hydrolyzed, resulting in unstable performance, and phosphate ester monomers are easily complexed with anti-rust paint fillers, resulting in gelation of the paint during storage.
[0008] Patent document CN118146424A discloses a self-drying high-gloss water-based acrylic emulsion for steel structure and its preparation method, comprising: component A: 60-70 parts of hard monomer, 30-40 parts of soft monomer, 20-25 parts of deionized water, 2-3 parts of anionic emulsifier, 1-1.5 parts of nonionic emulsifier, 0.05-0.1 parts of initiator; component B: 20-60 parts of hard monomer, 20-60 parts of soft monomer, 30-60 parts of functional monomer, 40-60 parts of deionized water, 2-3 parts of anionic emulsifier, 1-1.5 parts of nonionic emulsifier, 0-2 parts of molecular weight regulator; component C: 0.2-0.5 parts of anionic emulsifier, 0.1-1.3 parts of cationic emulsifier, 0. 002-0.005 parts of regulating buffer, 18-28 parts of deionized water; 5-10% of the mass ratio of component A pre-reacts with component C to generate free radicals and initiate polymerization; the functional monomer is any one or more of methacrylic acid, methacrylic acid hydroxyl monomer, methacrylic acid glycidyl ester, diacetone acrylamide, adipic acid dihydrazide; the hard monomer is any one or more of styrene, butyl methacrylate, methyl methacrylate; the soft monomer is any one or more of 2-ethylhexyl acrylate and butyl acrylate; the molecular weight regulator is α-methylstyrene linear dimer; the initiator is any one or more of ammonium persulfate and sodium persulfate; the regulating buffer includes sodium bicarbonate. However, the pH value of the document is too high, and the adhesion and corrosion resistance still cannot meet the requirements when used for galvanized steel sheets. Summary of the invention
[0009] The purpose of the present invention is to provide a water-based acrylic emulsion for galvanized steel coating and a production method thereof, so as to solve the problems of poor adhesion, corrosion resistance and storage stability existing in the prior art.
[0010] The purpose of the present invention is achieved through the following technical solutions:
[0011] The invention discloses a water-based acrylic emulsion for galvanized steel coating, which is prepared from the following raw materials in mass fraction: 1.0% to 2.0% of functional monomer, 9% to 15% of soft monomer, 15% to 20% of hard monomer, 0.05% to 0.15% of initiator, 0.4% to 0.7% of cationic emulsifier, 0.4% to 0.7% of nonionic emulsifier, 0.8% to 1.3% of isopropanol, 0.05% to 0.15% of pH value regulator, 0.1% to 0.5% of preservative, and the balance is deionized water;
[0012] The functional monomer is a mixture of at least one of hydroxyethyl acrylate, acrylic acid, ethylene glycol dimethacrylate (EGDMA), dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide, the mass ratio of the three being (3.0-5.0):(0.8-1.2):1, preferably (3.0-4.0):1:1;
[0013] The initiator is azobisisovaleronitrile, azobisisobutylamidine hydrochloride (AIBA, V50) and tert-butyl hydroperoxide in a mass ratio of (0.6-1.0):(2-3):1; the preferred ratio is 0.8:(2.3-2.6):1;
[0014] The soft monomer is isooctyl acrylate and / or butyl acrylate; the hard monomer is butyl methacrylate and / or methyl methacrylate;
[0015] The cationic emulsifier is hexadecyltrimethylammonium chloride, and the nonionic emulsifier is Clariant Emulsogen LCN 407 nonionic emulsifier;
[0016] The preservative is at least one of ascorbic acid and isothiazolin-based preservatives (such as Rohm and Haas preservative KATHON LXE); and the pH adjuster is formic acid.
[0017] A method for producing a water-based acrylic emulsion for galvanized steel coating of the present invention comprises the following steps:
[0018] S1, adding the nonionic emulsifier and 1 / 3 to 4 / 5 of the cationic emulsifier into an appropriate amount of deionized water, and stirring evenly; then adding the functional monomer, the soft monomer and the hard monomer thereto, stirring thoroughly for emulsification; then adding the initiator azobisisovaleronitrile, stirring evenly to obtain a pre-emulsion;
[0019] S2, add an appropriate amount of deionized water to the reactor, then add the remaining cationic emulsifier, stir and heat to 70-75° C. under nitrogen protection; first add 1 / 30-1 / 10 of the pre-emulsion to the reactor, then add azobisisobutylamidine hydrochloride; wait for the reactor to emit blue light, and keep the reaction at 73-78° C. for 15-30 minutes;
[0020] S3, adding the remaining pre-emulsion dropwise for 150 to 200 minutes, and then keeping the temperature at 73 to 78°C for 30 to 60 minutes;
[0021] S4, adding tert-butyl hydroperoxide as an initiator to the reactor dropwise for 10 to 20 minutes; after the addition is completed, keeping the temperature at 70 to 76° C. for 30 to 60 minutes;
[0022] S5, cooling to below 40° C., adding the pH adjuster to adjust the pH value to 4-5; and then adding the isopropanol and the preservative in sequence;
[0023] S6, adjusting the solid content to 28.0% to 32.0% with the remaining deionized water, filtering and discharging the material after the test is qualified, and obtaining a white water-based acrylic emulsion with a bluish glow.
[0024] Preferably, the cationic emulsifier is first dissolved in deionized water at 35-45° C. before use.
[0025] Preferably, the initiator tert-butyl hydroperoxide has a dropping rate of 0.8 to 1.5 kg / min.
[0026] Preferably, when the preservative comprises ascorbic acid, the step S4 comprises: adding tert-butyl hydroperoxide as an initiator to the reactor dropwise for 10 to 20 minutes; adding ascorbic acid dropwise for 30 to 50 minutes; and after the addition is completed, keeping the reaction at 70 to 76° C. for 30 to 60 minutes.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] The present invention adopts dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide, which are functional acrylate monomers containing amino groups, for compounding and copolymerizing, so that the water-based acrylic emulsion of the present invention has a self-curing function; the cross-linking degree of the emulsion molecules is improved, thereby improving the adhesion, water resistance and salt spray resistance of the coating film, and ensuring the anti-corrosion effect; the optimized combination of three initiators also has a positive effect on the storage stability and the anti-corrosion effect, so that the water-based acrylic emulsion used for galvanized steel coating has excellent adhesion and corrosion resistance, improves the sealing property of the film after the emulsion is coated, and can meet the requirements of galvanized steel coating. DETAILED DESCRIPTION
[0029] The present invention is further described below by means of specific embodiments, which are only used to illustrate the present invention rather than to limit the present invention.
[0030] Example 1
[0031] The water-based acrylic emulsions for galvanized steel coatings of Examples 1 to 3 and Comparative Examples 1 to 3 have a formula as shown in Table 1, and the production method thereof comprises the following steps:
[0032] S1, adding a nonionic emulsifier and 4 / 5 of a cationic emulsifier to an appropriate amount of deionized water, and stirring evenly; then adding a functional monomer, a soft monomer, and a hard monomer thereto, stirring and emulsifying thoroughly; then adding an initiator, azobisisovaleronitrile, and stirring evenly to obtain a pre-emulsified liquid;
[0033] S2, add an appropriate amount of deionized water to the reactor, then add the remaining cationic emulsifier, stir and heat to 75°C under nitrogen protection; first add 1 / 20 of the pre-emulsified liquid to the reactor, then add azobisisobutylamidine hydrochloride; wait for the reactor to emit blue light, and keep the reaction at 73-78°C for 20 minutes;
[0034] S3, adding the remaining pre-emulsion dropwise for 180 min, and then keeping the temperature at 73-78°C for 45 min;
[0035] S4, add tert-butyl hydroperoxide to the reaction kettle dropwise for 20 minutes; add ascorbic acid dropwise for 40 minutes; after the addition is completed, keep the temperature at 70-76° C. for 50 minutes;
[0036] S5, cooling to below 40°C, adding a pH adjuster to adjust the pH value to 4.5; and then adding isopropyl alcohol and a preservative in sequence;
[0037] S6, adjusting the solid content to 30.0% with the remaining deionized water, filtering and discharging the material after the test is qualified, and obtaining a white water-based acrylic emulsion with a bluish glow.
[0038] Table 1 Raw materials and proportions of Examples 1 to 3 and Comparative Examples 1 to 3, unit: wt%
[0039]
[0040]
[0041] Comparative Example 1 is a comparative example of Example 1, except that the functional monomer dimethylaminopropyl acrylamide is not added in Comparative Example 1.
[0042] Comparative Example 2 is a comparative example of Example 1, except that in Comparative Example 2, the functional monomers dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide are not added.
[0043] Comparative Example 3 is a comparative example of Example 1, except that the added amounts of azobisisovaleronitrile and azobisisobutylamidine hydrochloride are interchanged in Comparative Example 3.
[0044] The water-based acrylic emulsions obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were tested. The three embodiments and three comparative examples of the water-based acrylic emulsions of the present invention were applied to water-based coatings, which included the following components: 50 parts of water-based acrylic emulsions, 30 parts of color paste, 2 parts of film-forming agent, and 1 part of water-based leveling agent. Adhesion was measured according to the cross-hatch method. Water resistance (coating thickness 18 μm) was measured according to the provisions of 5.1 of "GB-T1733-1993 Paint Film Water Resistance Test Method", immersed in grade 3 water that meets the requirements of GB / T6682, and the sample was taken out for observation after the specified time, and the results were evaluated according to the provisions of GB / T1766-2008. The salt spray resistance (coating thickness 18μm) shall be measured according to the provisions of 5.4 of GB / T1771-2007 Determination of neutral salt spray resistance of paints and varnishes. If blistering, rusting, cracking and peeling of the paint film occur, the results shall be evaluated according to the provisions of GB / T1766-2008.
[0045] Table 2 Test results of Examples 1 to 3 and Comparative Examples 1 to 3
[0046]
[0047] As can be seen from Table 2, the present invention adopts the amino-containing functional acrylate monomers dimethylaminoethyl methacrylate and dimethylaminopropyl acrylamide for compound copolymerization, which improves the crosslinking degree of the emulsion molecules, thereby improving the adhesion, water resistance and salt spray resistance of the coating film, and ensuring the anti-corrosion effect; the optimized combination of the three initiators also has a positive effect on the storage stability and anti-corrosion effect.
Claims
1. A water-based acrylic emulsion for galvanized steel coating, characterized in that: The invention is prepared from the following raw materials in mass fraction: 1.0% to 2.0% functional monomer, 9% to 15% soft monomer, 15% to 20% hard monomer, 0.05% to 0.15% initiator, 0.4% to 0.7% cationic emulsifier, 0.4% to 0.7% nonionic emulsifier, 0.8% to 1.3% isopropyl alcohol, 0.05% to 0.15% pH regulator, 0.1% to 0.5% preservative, and the balance is deionized water; the functional monomer is a mixture of at least one of hydroxyethyl acrylate, acrylic acid, and ethylene glycol dimethacrylate, dimethylaminoethyl methacrylate, and dimethylaminopropyl acrylamide, and the mass ratio of the three is (3.0 to 5.0):(0.8 to 1.2):
1.
2. The aqueous acrylic emulsion for galvanized steel coating according to claim 1, characterized in that The initiator is azobisisovaleronitrile, azobisisobutylamidine hydrochloride and tert-butyl hydroperoxide in a mass ratio of (0.6-1.0):(2-3):
1.
3. The aqueous acrylic emulsion for galvanized steel coating according to claim 1, characterized in that The soft monomer is isooctyl acrylate and / or butyl acrylate; the hard monomer is butyl methacrylate and / or methyl methacrylate.
4. The aqueous acrylic emulsion for galvanized steel coating according to claim 1, wherein The cationic emulsifier is cetyltrimethylammonium chloride, and the nonionic emulsifier is Clariant Emulsogen LCN 407 nonionic emulsifier.
5. The aqueous acrylic emulsion for galvanized steel coating according to claim 1, characterized in that The preservative is at least one of ascorbic acid and isothiazolinyl preservatives; and the pH adjuster is formic acid.
6. The method for producing a water-based acrylic emulsion for galvanized steel coating according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, adding the nonionic emulsifier and 1 / 3 to 4 / 5 of the cationic emulsifier to an appropriate amount of deionized water and stirring evenly; then adding the functional monomer, soft monomer and hard monomer thereto and stirring thoroughly to emulsify; then adding azobisisovaleronitrile as an initiator and stirring evenly to obtain a pre-emulsion; S2, adding an appropriate amount of deionized water to the reactor, then adding the remaining cationic emulsifier, stirring and heating to 70-75° C. under nitrogen protection; first adding 1 / 30-1 / 10 of the pre-emulsion to the reactor, then adding azobisisobutylamidine hydrochloride; after the reactor appears blue light, keep the reaction at 73-78° C. for 15-30 minutes; S3, adding the remaining pre-emulsion dropwise for 150-200 min, and then keeping the temperature at 73-78°C for 30-60 min; S4, adding tert-butyl hydroperoxide as an initiator dropwise to the reactor for 10 to 20 minutes; and maintaining the reaction temperature at 70 to 76° C. for 30 to 60 minutes after the addition is complete; S5, cooling to below 40° C., adding the pH adjuster to adjust the pH to 4-5; and then sequentially adding the isopropyl alcohol and preservative; S6, adjust the solid content to 28.0% to 32.0% with the remaining deionized water, filter and discharge the material after passing the test to obtain a white water-based acrylic emulsion with a bluish glow.
7. The method for producing a water-based acrylic emulsion for galvanized steel coating according to claim 6, wherein: The cationic emulsifier is first dissolved in deionized water at 35-45° C. before use.
8. The method for producing the water-based acrylic emulsion for galvanized steel coating according to claim 6, wherein: The initiator tert-butyl hydroperoxide is added at a rate of 0.8 to 1.5 kg / min.
9. The method for producing a water-based acrylic emulsion for galvanized steel coating according to claim 6, wherein: When the preservative includes ascorbic acid, the step S4 comprises: adding tert-butyl hydroperoxide as an initiator dropwise to the reactor for 10 to 20 minutes; adding ascorbic acid dropwise for 30 to 50 minutes; and after the addition is completed, keeping the reaction at 70 to 76° C. for 30 to 60 minutes.
Citation Information
Patent Citations
Air-drying highlight water-based acrylic emulsion for steel structure and preparation method of air-drying highlight water-based acrylic emulsion
CN118146424A