Polylactic acid composite membrane material as well as preparation method and application thereof

Through the combination of polylactic acid polyols, isocyanates and other materials and specific reaction steps, the toughness and ductility of polylactic acid composite film materials are improved, and its shortcomings in packaging field are solved, achieving high light transmission and complete degradability are achieved. effect.

CN119081058APending Publication Date: 2024-12-06NORTHEAST FORESTRY UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411369198.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polylactic acid packaging film materials have insufficient toughness and ductility, making it difficult to apply in packaging fields that require certain flexibility.

Method used

The polylactic acid composite film material is prepared by specific reaction steps using a combination of polylactic acid polyol, isocyanate, anhydrous organic solvent, catalyst and chain extender to increase its toughness and ductility.

Benefits of technology

The prepared polylactic acid composite film material has high light transmittance, high tensile strength and elongation of break, is suitable for soft packaging, and has fully degradable properties to replace petroleum-based polyethylene materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081058A_ABST
    Figure CN119081058A_ABST
Patent Text Reader

Abstract

The invention relates to a polylactic acid composite film material as well as a preparation method and application thereof, and belongs to the technical field of polymer packaging films. In order to solve the problems of poor toughness and poor ductility of the existing polylactic acid packaging film material, the invention provides a polylactic acid composite film material which comprises the following components: polylactic acid polyol, isocyanate, an anhydrous organic solvent, a catalyst and a chain extender. The polylactic acid composite film has high toughness and ductility while having good light transmittance, the light transmittance of the polylactic acid composite film reaches 83% or above, the highest elongation at break can reach 417%, and the polylactic acid composite film can be well applied to the field of flexible packaging. By adding the chain extender, the toughness of the composite membrane material is further improved, and the tensile strength of the composite membrane material can reach 32.9 Mpa to the maximum. The polylactic acid composite film disclosed by the invention has the characteristic of complete degradability, and can replace materials such as petroleum-based polyethylene to be applied to the field of plastic packaging. The preparation process is simple, low in cost and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer packaging films, and in particular relates to a polylactic acid composite film material and a preparation method and application thereof. Background Art

[0002] Petroleum-based plastic packaging materials are known for their rich raw materials and mature production processes. They have obvious advantages in production costs, water resistance, durability, processing, corrosion resistance and insulation. However, they are difficult to decompose in the natural environment, causing long-term pollution to soil and water bodies and affecting ecological balance. It is often difficult to effectively classify petroleum-based plastic packaging materials when recycling them, and incineration will also release toxic and harmful gases, posing a threat to the environment and human health. Therefore, it is necessary to develop more environmentally friendly and sustainable alternative materials.

[0003] Polylactic acid (PLA) packaging film, as a new type of environmentally friendly green biodegradable material, has received widespread attention and application in recent years. This packaging film uses lactic acid as the main raw material and is made through polycondensation reaction. It not only has good physical and chemical properties, but also has a variety of unique advantages and characteristics, making it occupy an important position in the packaging industry. However, in actual applications, polylactic acid packaging film materials have the problems of poor toughness and ductility. The packaging film is easy to break when subjected to slight external force or deformation, which limits its application in packaging fields that require a certain degree of ductility or flexibility. Summary of the invention

[0004] In order to solve the problems of poor toughness and ductility of existing polylactic acid packaging film materials, the present invention provides a polylactic acid composite film material and a preparation method and application thereof.

[0005] The technical solution of the present invention:

[0006] A polylactic acid composite film material comprises polylactic acid polyol, isocyanate, anhydrous organic solvent, catalyst and chain extender; wherein the mass volume ratio of polylactic acid polyol, isocyanate, anhydrous organic solvent and chain extender is 8-10g:1-3g:80-120ml:0.1-1.5g, and the amount of the catalyst is 0.3% of the total mass of the polylactic acid polyol and isocyanate.

[0007] Furthermore, the polylactic acid polyol is one or a combination of polylactic acid polyols having a molecular weight of 500 to 2000.

[0008] Further, the isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate TDI, isophorone diisocyanate IPDI, diphenylmethane diisocyanate MDI, dicyclohexylmethane diisocyanate HMDI, hexamethylene diisocyanate HDI or lysine diisocyanate.

[0009] Furthermore, the anhydrous organic solvent is one of butanone, dioxane, N,N-dimethylformamide, dimethylacetamide or dimethyl sulfoxide.

[0010] Furthermore, the catalyst is a tin-based catalyst, specifically stannous octoate or stannous chloride.

[0011] Furthermore, the chain extender is one or a combination of isophthalic acid hydrazide, sebacic acid hydrazide, succinic acid dihydrazide or 2,5-bis(benzyloxy)terephthaloylhydrazide.

[0012] A method for preparing a polylactic acid composite film material comprises the following steps:

[0013] Step 1, placing polylactic acid polyol, isocyanate and catalyst under an inert atmosphere, reacting at a certain temperature for a certain time to obtain a prepolymer;

[0014] Step 2: adding an anhydrous organic solvent and a chain extender to the prepolymer obtained in step 1, lowering the reaction temperature to room temperature and continuing the reaction for a certain period of time under an inert atmosphere to obtain a composite system;

[0015] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature, and volatilize and remove the anhydrous organic solvent in the composite system to obtain a polylactic acid composite film material.

[0016] Furthermore, in step 1, the reaction temperature is 70-90° C., and the reaction time is 3-5 h.

[0017] Furthermore, the reaction time in step 2 is 12 to 48 hours.

[0018] Furthermore, the thickness of the polylactic acid composite film material obtained in step three is 0.02 to 2 mm.

[0019] Beneficial effects of the present invention:

[0020] The polylactic acid composite film provided by the present invention has good light transmittance and high toughness and ductility, with a light transmittance of more than 83% and a maximum elongation at break of 417%, and can be well applied in the field of flexible packaging. The present invention further improves the toughness of the composite film material by adding a chain extender, so that its tensile strength can reach up to 32.9Mpa.

[0021] The polylactic acid composite film provided by the present invention has the characteristic of being completely degradable, and can replace materials such as petroleum-based polyethylene and be applied to the field of plastic packaging. The preparation process of the polylactic acid composite film of the present invention is simple, the cost is low, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1This is a real photo of the polylactic acid composite film material prepared by the present invention;

[0023] Figure 2 A comparison chart of the tensile strength of the polylactic acid composite film materials prepared in Examples 1 to 4;

[0024] Figure 3 A comparison chart of the elongation at break of the polylactic acid composite film materials prepared in Examples 1 to 4;

[0025] Figure 4 It is a stress-strain curve diagram of the polylactic acid composite film material prepared in Example 1 to Example 4. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.

[0027] Example 1

[0028] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0029] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are isophorone diisocyanate IPDI, butanone, stannous octoate and isophthalic acid hydrazide IPDH.

[0030] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0031] Step 1: First weigh 8.02g PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.62g IPDI, add polylactic acid polyol and 0.3% stannous octoate of the total mass of isocyanate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0032] Step 2: Add 100 ml of butanone to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system, cool the system to room temperature of 25°C, then add 0.69 g of IPDH to carry out chain extension reaction, and react for 12 hours with nitrogen throughout the process to obtain a composite system.

[0033] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into a 50° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0034] Example 2

[0035] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0036] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are isophorone diisocyanate IPD, butanone, stannous octoate and isophthalic acid hydrazide IPDH.

[0037] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0038] Step 1: First weigh 8.09g PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.32g IPDI, add polylactic acid polyol and 0.3% stannous octoate of the total mass of isocyanate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0039] Step 2: Add 100 ml of butanone to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system, cool the system to room temperature 25°C, then add 0.42 g of IPDH to carry out chain extension reaction, and react for 12 hours with nitrogen throughout the process to obtain a composite system.

[0040] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into a 50° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0041] Example 3

[0042] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0043] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are isophorone diisocyanate IPDI, butanone, stannous octoate and isophthalic acid hydrazide IPDH.

[0044] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0045] Step 1: First weigh 8.50g PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.62g IPDI, add polylactic acid polyol and 0.3% stannous octoate of the total mass of isocyanate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0046] Step 2: Add 100 ml of butanone to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system, cool the system to room temperature 25°C, then add 0.25 g of IPDH to carry out chain extension reaction, and react for 12 hours with nitrogen throughout the process to obtain a composite system.

[0047] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into a 50° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0048] Example 4

[0049] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0050] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are isophorone diisocyanate IPDI, butanone, stannous octoate and isophthalic acid hydrazide IPDH.

[0051] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0052] Step 1: First weigh 8.82g PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.03g IPDI, add polylactic acid polyol and 0.3% stannous octoate of the total mass of isocyanate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0053] Step 2: Add 100 ml of butanone to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system, cool the system to room temperature of 25°C, then add 0.11 g of IPDH to carry out chain extension reaction, and react for 12 hours with nitrogen throughout the process to obtain a composite system.

[0054] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into a 50° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0055] Example 5

[0056] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0057] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 1000, and the other components are toluene diisocyanate, dioxane, stannous octoate and sebacic acid hydrazide.

[0058] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0059] Step 1: First weigh 8.42g of polylactic acid diol PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.10g of toluene diisocyanate, add polylactic acid polyol and 0.3% of the total mass of isocyanate stannous octoate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0060] Step 2: Add 100 ml of dioxane to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system, cool the system to room temperature (25°C), then add 0.48 g of sebacic acid hydrazide to carry out chain extension reaction, and react for 12 hours with nitrogen gas throughout the process to obtain a composite system.

[0061] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into an 80° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0062] Example 6

[0063] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0064] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 1000, and the other components are diphenylmethane diisocyanate, N,N-dimethylformamide, stannous octoate and succinic acid dihydrazide.

[0065] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0066] Step 1: First weigh 8.26g of polylactic acid diol PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 1.29g of diphenylmethane diisocyanate, add 0.3% of the total mass of polylactic acid polyol and isocyanate stannous octoate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0067] Step 2: Add 100 ml of N,N-dimethylformamide to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system. After cooling the system to room temperature of 25°C, add 0.45 g of succinic acid dihydrazide to carry out chain extension reaction. React for 12 hours with nitrogen gas throughout the process to obtain a composite system.

[0068] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into an 80° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0069] Example 7

[0070] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0071] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are dicyclohexylmethane diisocyanate, dimethylacetamide, stannous octoate and 2,5-bis(benzyloxy)terephthaloylhydrazide.

[0072] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0073] Step 1: First weigh 8.62g of polylactic acid diol PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 0.57g of dicyclohexylmethane diisocyanate, add 0.3% of the total mass of polylactic acid polyol and isocyanate stannous octoate, pass nitrogen, react at 80°C for 3.5h to obtain a prepolymer.

[0074] Step 2: Add 100 ml of dimethylacetamide to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system. After the system is cooled to room temperature of 25° C., 0.82 g of 2,5-bis(benzyloxy)terephthaloylhydrazide is added to carry out a chain extension reaction. Nitrogen is passed throughout the reaction for 12 hours to obtain a composite system.

[0075] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into an 80° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0076] Example 8

[0077] This embodiment provides a polylactic acid composite film material and a preparation method thereof.

[0078] In the components of the polylactic acid composite film material in this embodiment, the polylactic acid polyol is polylactic acid diol PLA-OH with a molecular weight of 2000, and the other components are hexamethylene diisocyanate, dimethyl sulfoxide, stannous chloride and sebacic acid hydrazide.

[0079] This embodiment provides a method for preparing a polylactic acid composite film material, comprising the following steps:

[0080] Step 1: First weigh 9.09 g of polylactic acid diol PLA-OH in a four-necked flask connected to a vacuum pump, stir to remove moisture, add 0.38 g of hexamethylene diisocyanate, add 0.3% of the total mass of polylactic acid polyol and isocyanate stannous octoate, pass nitrogen, react at 80°C for 3.5 hours to obtain a prepolymer.

[0081] Step 2: Add 100 ml of dimethyl sulfoxide to the prepolymer obtained in step 1 to reduce the viscosity of the reaction system. After the system is cooled to room temperature of 25° C., 0.52 g of sebacic acid hydrazide is added to carry out a chain extension reaction. Nitrogen is passed throughout the reaction for 12 hours to obtain a composite system.

[0082] Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature overnight, and then put it into an 80° C. oven for 24 hours to volatilize and remove butanone in the composite system, thereby obtaining a polylactic acid composite film material with a thickness of 0.2 mm.

[0083] Figure 1 This is a real photo of the polylactic acid composite film material prepared by the present invention; the picture shows that the polylactic acid composite film material has good light transmittance, and its light transmittance reaches more than 83%, which meets the requirements of the packaging material field for film transmittance.

[0084] Figure 2 This is a comparison chart of the tensile strength of the polylactic acid composite film materials prepared in Examples 1 to 4. The tensile strength of the polylactic acid composite film material prepared in Example 1 is 29.90±2.09MPa, the tensile strength of the polylactic acid composite film material prepared in Example 2 is 28.25±8.46MPa, the tensile strength of the polylactic acid composite film material prepared in Example 3 is 32.90±2.02MPa, and the tensile strength of the polylactic acid composite film material prepared in Example 4 is 18.93±3.57MPa. It can be seen that the polylactic acid composite film material prepared by the present invention has good tensile properties.

[0085] Figure 3 This is a comparison chart of the elongation at break of the polylactic acid composite film materials prepared in Examples 1 to 4. The elongation at break of the polylactic acid composite film material prepared in Example 1 is 285.43%, the elongation at break of the polylactic acid composite film material prepared in Example 2 is 331.12%, the elongation at break of the polylactic acid composite film material prepared in Example 3 is 328.09%, and the elongation at break of the polylactic acid composite film material prepared in Example 4 is 417.95%. It can be seen that the polylactic acid composite film material prepared by the present invention has good elongation at break.

[0086] Figure 4The stress-strain curves of the polylactic acid composite film materials prepared in Examples 1 to 4 show that the polylactic acid composite film materials prepared in the present invention exhibit a relatively long plastic deformation stage, and can still maintain a certain upward trend after reaching the tensile strength, showing good toughness and ductility.

Claims

1. A polylactic acid composite film material, characterized in that: The components include polylactic acid polyol, isocyanate, anhydrous organic solvent, catalyst and chain extender; wherein the mass volume ratio of polylactic acid polyol, isocyanate, anhydrous organic solvent and chain extender is 8-10g:1-3g:80-120ml:0.1-1.5g, and the amount of the catalyst is 0.3% of the total mass of polylactic acid polyol and isocyanate.

2. A polylactic acid composite film material according to claim 1, characterized in that: The polylactic acid polyol is one or a combination of polylactic acid polyols having a molecular weight of 500 to 2000.

3. A polylactic acid composite film material according to claim 1 or 2, characterized in that: The isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate.

4. A polylactic acid composite film material according to claim 3, characterized in that: The anhydrous organic solvent is one of butanone, dioxane, N,N-dimethylformamide, dimethylacetamide or dimethyl sulfoxide.

5. A polylactic acid composite film material according to claim 4, characterized in that: The catalyst is a tin-based catalyst, specifically stannous octoate or stannous chloride.

6. A polylactic acid composite film material according to claim 5, characterized in that: The chain extender is one or a combination of isophthalic acid hydrazide, sebacic acid hydrazide, succinic acid dihydrazide or 2,5-bis(benzyloxy)terephthaloylhydrazide.

7. A method for preparing a polylactic acid composite film material according to any one of claims 1 to 6, characterized in that: The steps include: Step 1, placing polylactic acid polyol, isocyanate and catalyst under an inert atmosphere, reacting at a certain temperature for a certain time to obtain a prepolymer; Step 2: adding an anhydrous organic solvent and a chain extender to the prepolymer obtained in step 1, lowering the reaction temperature to room temperature and continuing the reaction for a certain period of time under an inert atmosphere to obtain a composite system; Step 3: pour the composite system obtained in step 2 into a mold, let it stand at room temperature, and volatilize and remove the anhydrous organic solvent in the composite system to obtain a polylactic acid composite film material.

8. The method for preparing the polylactic acid composite film material according to claim 7, characterized in that: In step 1, the reaction temperature is 70-90° C. and the reaction time is 3-5 h.

9. The method for preparing the polylactic acid composite film material according to claim 7 or 8, characterized in that: The reaction time in step 2 is 12 to 48 hours.

10. The method for preparing the polylactic acid composite film material according to claim 9, characterized in that: The thickness of the polylactic acid composite film material obtained in step 3 is 0.02 to 2 mm.

Citation Information

Patent Citations

  • Polylactic acid based polyurethane elastomer material for medical infusion apparatus and preparation method thereof

    CN105175676A

  • Polylactic acid-based thermoplastic polyurethane elastomer material and preparation method thereof

    CN110627985A

  • Bio-based high-damping thermoplastic polyurethane elastomer material as well as preparation method and application thereof

    CN115260433A

  • Self-repairing waterborne polyurethane film and preparation method thereof

    CN116355249A