Anti-ultraviolet polyurethane composite material and preparation method thereof

By using zinc oxide precursor solution for in-situ synthesis and polystyrene grafting technology in polyurethane coatings, uniformly dispersed zinc oxide particles are formed, and the problem of insufficient microbial reproduction and ultraviolet resistance of polyurethane coatings after collision is solved. It significantly improves antibacterial and UV resistance and extends the service life of the coating.

CN119081066APending Publication Date: 2024-12-06LISHUI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123787.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

After being impacted or scratched, the polyurethane coating has problems such as microorganisms entering and reproduction, resulting in a decrease in service life and insufficient UV resistance.

Method used

In-situ synthesis is performed using zinc oxide precursor solution, combined with polystyrene grafting technology, uniformly dispersed zinc oxide particles are formed to enhance antibacterial and ultraviolet resistance.

Benefits of technology

Through uniformly dispersed zinc oxide particles, the antibacterial and UV resistance of polyurethane composites is significantly improved, extending the service life of the coating and improving its protective effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995791460000101
    Figure BDA0004995791460000101
  • Figure BDA0004995791460000102
    Figure BDA0004995791460000102
Patent Text Reader

Abstract

The invention relates to the field of coating materials, and particularly discloses an anti-ultraviolet polyurethane composite material and a preparation method thereof. The invention relates to an anti-ultraviolet polyurethane composite material, which is prepared from 2 to 3 mol of dimer acid diisocyanate, 0.6 to 1 mol of polypropylene carbonate glycol, 0.1 to 0.4 mol of siloxane modified polyether, 0.4 to 2 mol of isophorone diamine, 0.4 to 2 mol of polyether amine D-230 and 0.25 to 0.5 mol / L of zinc oxide precursor solution, wherein the zinc oxide precursor solution is used for in-situ synthesis of zinc oxide polyurethane; the preparation method comprises the following steps: carrying out in-situ synthesis on a zinc oxide precursor solution grafted with polystyrene and a polyurethane polymer through an in-situ synthesis method to obtain a zinc oxide precursor solution; the uvioresistant polyurethane composite material disclosed by the invention has the advantages of excellent uvioresistant performance and antibacterial performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coating materials, and more specifically, to an anti-ultraviolet polyurethane composite material and a preparation method thereof. Background Art

[0002] Polyurethane (PU) is a general term for block copolymers containing a large number of repeated carbamate groups (-NHCOO-). From the perspective of molecular structure, the polyurethane molecular chain is composed of soft segments and hard segments that are continuously arranged alternately. The unique block copolymer structure gives PU extremely high tensile strength, high elasticity, oil resistance, wear resistance, flexible design and easy processing. It is widely used in elastomers, resins, coatings, adhesives, fibers and other fields.

[0003] However, during the use of the polyurethane coating, it will inevitably be hit or scratched, which will directly affect the safety and service life of the polyurethane coating. In order to solve this problem, making the polyurethane coating self-healing is currently one of the effective methods.

[0004] Although the above-mentioned self-healing polyurethane coating can self-recover after collision or scratch, the attached microorganisms will also enter the self-healing polyurethane coating during collision or scratch. The main raw material of the self-healing polyurethane coating is bio-based, and there is a situation of large-scale reproduction of microorganisms, which will cause the service life of the self-healing polyurethane coating after collision or scratch to be significantly reduced. Summary of the invention

[0005] In order to improve the defect that the anti-ultraviolet performance of polyurethane is still insufficient, the present application provides an anti-ultraviolet polyurethane composite material and a preparation method thereof.

[0006] In the first aspect, the present application provides an anti-ultraviolet polyurethane composite material, which adopts the following technical solution:

[0007] An anti-ultraviolet polyurethane composite material and a preparation method thereof, comprising the following raw materials: 2-3 mol dimer acid diisocyanate, 0.6-1 mol polypropylene carbonate diol, 0.1-0.4 mol siloxane modified polyether, 0.4-2 mol isophorone diamine, 0.4-2 mol polyetheramine D-230 and 0.25-0.5 mol / L zinc oxide precursor solution, wherein the zinc oxide precursor solution is used for in-situ synthesis of zinc oxide polyurethane.

[0008] Because zinc oxide has a high refractive index, it can effectively scatter and reflect ultraviolet rays and absorb ultraviolet photons in the UVA and UVB bands, converting their energy into heat energy. At the same time, zinc oxide can release zinc ions, which can combine with proteins and enzymes on the bacterial cell walls to destroy their structure and function. At the same time, it can induce oxidative stress in bacterial cells, thereby damaging bacterial DNA and proteins and inhibiting bacterial growth and reproduction.

[0009] However, conventional zinc oxide has a high surface energy, irregular particle shape, strong interaction between particles due to surface charge and polarity, is easily aggregated to form agglomerates, and has weak interaction in non-polar or low-order media, so its ability to be evenly dispersed is insufficient. Since the zinc oxide precursor solution used in the present application is used for the in-situ synthesis of zinc oxide polyurethane, the zinc oxide particles are formed simultaneously during the polyurethane polymerization process, and the particles can be evenly distributed in the polymer matrix at the initial stage of formation, which is beneficial to the stable dispersion of zinc oxide, thereby enabling the prepared polyurethane composite material to have better antibacterial and anti-ultraviolet properties.

[0010] Preferably, the zinc oxide precursor solution is prepared using zinc acetate as a zinc source.

[0011] Preferably, the zinc oxide precursor solution contains polystyrene.

[0012] Although the in-situ synthesis method can effectively improve the dispersibility of zinc oxide, improper control of the reaction conditions and post-treatment during the in-situ synthesis may also lead to agglomeration between particles, making the dispersion effect of zinc oxide still insufficient.

[0013] Polystyrene can be used as a carrier to adsorb or embed zinc oxide into its matrix, so that a protective layer is formed on the surface of zinc oxide, allowing zinc oxide to be dispersed in the polystyrene matrix. Polystyrene can also reduce the interfacial tension between zinc oxide and the solvent, making zinc oxide more easily wetted. The improvement in wettability is conducive to better dispersion of zinc oxide in the solvent. Therefore, polystyrene is added to the zinc oxide precursor solution to improve the dispersibility of zinc oxide.

[0014] Preferably, the zinc oxide precursor solution is a polystyrene grafted vinyl zinc salt solution.

[0015] Since polystyrene and zinc oxide are added separately, there is a situation where the reaction between polystyrene and zinc oxide is hindered by other components, which makes it impossible for polystyrene to disperse and modify zinc oxide, thereby causing the anti-ultraviolet performance of zinc oxide to be insufficient.

[0016] Compared with adding polystyrene and zinc oxide separately, pre-connecting polystyrene with zinc oxide by grafting effectively reduces the possibility of obstruction between polystyrene and zinc oxide by other components, thereby promoting better dispersion of zinc oxide, and ultimately resulting in better UV resistance of the polyurethane composite material.

[0017] Preferably, the preparation method of the vinyl zinc salt solution is as follows: 1 mol of zinc acetate is weighed and put into deionized water, and after stirring, suction filtering is performed, the filtered zinc acetate is put into a vacuum drying oven for drying, and the vacuum-dried zinc acetate is added to an anhydrous ethanol solution containing 1.2 mol of vinyl triethoxysilane, and after the reaction is completed, it is washed with anhydrous ethanol, and then the anhydrous ethanol is washed away with deionized water to obtain a modified vinyl zinc salt solution.

[0018] Since zinc acetate is a metal salt, it usually dissociates into zinc ions and acetate ions in solution. These ions themselves do not have the activity to directly initiate the polystyrene grafting reaction. The grafting reaction usually requires active species such as free radicals, cations or anions to attack the polystyrene molecular chain.

[0019] A modified vinyl zinc salt solution is obtained by adding vinyl triethoxysilane to zinc acetate. Vinyl triethoxysilane is an organic silicon compound containing vinyl and silane groups, so that zinc acetate can react with the vinyl group in vinyl triethoxysilane to obtain a modified vinyl zinc salt solution.

[0020] Preferably, the preparation method of the zinc oxide precursor solution is as follows: styrene and initiator BPO are added to a polymerization bottle, and then a vinyl zinc salt solution is added. After vacuuming and nitrogen replacement, the bottle mouth is sealed and the polymerization bottle is placed in an oil bath. The reaction is stirred at 60° C. for 4-6 hours. After the reaction, deionized water is added and the zinc oxide precursor solution is obtained by ultrasonic dissolution.

[0021] In common synthesis methods, the nucleation and growth process of zinc oxide may not be strictly controlled, resulting in uneven particle size and irregular shape, which makes it easy for particles to agglomerate. During the synthesis process, it is usually necessary to proceed at high temperature. High temperature treatment may also lead to reduced dispersibility of zinc oxide.

[0022] However, the in-situ synthesis method allows the nucleation and growth process of zinc oxide to be controlled under specific conditions, and the formation of zinc oxide can be manipulated at the atomic or molecular level to obtain uniformly dispersed particles. At the same time, the in-situ synthesis method is usually carried out under relatively mild conditions, which helps to form uniform and well-dispersed zinc oxide.

[0023] Preferably, the raw materials include: 0.9-1.1 mol zinc acetate, 1.1-1.3 mol vinyltriethoxysilane, 1.1-1.3 mol styrene and 0.009-0.02 mol initiator BPO.

[0024] Since the performance of the grafting reaction may be relatively low when the added amounts of zinc acetate, vinyl triethoxysilane and styrene are the same, in this application the added amount of styrene and vinyl triethoxysilane is greater than the added amount of zinc acetate, which is beneficial to improving the performance of the grafting reaction, making the reaction more complete and the grafting density higher.

[0025] In a second aspect, the present application provides a method for preparing an anti-ultraviolet polyurethane composite material, which adopts the following technical solution:

[0026] A method for preparing an anti-ultraviolet polyurethane composite material comprises the following steps:

[0027] S1: Weigh allyl glycidyl ether and place it in a four-necked flask, add isopropanol solution of platinum tetrachloride as a reaction catalyst, heat to 90°C, stir for 0.5h to complete activation, slowly drop heptamethyltrisiloxane and react for 4h, remove impurities, and obtain siloxane-modified glycidyl ether;

[0028] S2: Add siloxane-modified glycidyl ether, initiator diethylene glycol and catalyst boron trifluoride·ethyl ether into a flask, heat to 60°C and react for 0.5h to complete activation, cool to 5°C in an ice-water bath, slowly add propylene oxide dropwise into the flask, stir and react for 5h to obtain siloxane-modified polyether;

[0029] S3: Weigh a mixture of polypropylene carbonate diol and a small amount of siloxane-modified polyether and add it to a four-necked flask, vacuum dehydrate at 120-130° C. for 2 h, then cool to 80° C., add dimer acid diisocyanate and catalyst dibutyltin dilaurate, and react for 3 h to obtain a polyurethane prepolymer;

[0030] S4: Add a mixture of 2-4 parts by mass of ethanol and 120-140 parts by mass of acetone to the polyurethane prepolymer, add the zinc oxide precursor solution and the emulsifier, continue to stir at 50-60°C for 0.5-1h for emulsification, then evaporate the acetone at 94°C under normal pressure until no odor is detected, cool to room temperature, add water to dilute to the required concentration, and obtain an in-situ synthesized zinc oxide polyurethane solution;

[0031] S5: Then, tetrahydrofuran was added to dissolve, cooled to 10°C with ice water, and isophorone diamine and polyetheramine D-230 were slowly added dropwise. After the addition was completed, the mixture was stirred and reacted for 3 hours;

[0032] S6: Pour the zinc oxide polyurethane solution into a polytetrafluoroethylene mold and place it in a fume hood to air dry to obtain a zinc oxide polyurethane elastomer.

[0033] In summary, this application has the following beneficial effects:

[0034] 1. Because zinc oxide has a high refractive index, it can effectively scatter and reflect ultraviolet rays and absorb ultraviolet photons in the UVA and UVB bands, converting their energy into heat energy. At the same time, zinc oxide can release zinc ions, which can combine with proteins and enzymes on the bacterial cell walls to destroy their structure and function. At the same time, it can induce oxidative stress in bacterial cells, thereby damaging bacterial DNA and proteins and inhibiting bacterial growth and reproduction.

[0035] However, conventional zinc oxide has a high surface energy, irregular particle shape, strong interaction between particles due to surface charge and polarity, is easily aggregated to form agglomerates, and has weak interaction in non-polar or low-order media, so its ability to be evenly dispersed is insufficient. Since the zinc oxide precursor solution used in the present application is used for the in-situ synthesis of zinc oxide polyurethane, the zinc oxide particles are formed simultaneously during the polyurethane polymerization process, and the particles can be evenly distributed in the polymer matrix at the initial stage of formation, which is beneficial to the stable dispersion of zinc oxide, thereby enabling the prepared polyurethane composite material to have better antibacterial and anti-ultraviolet properties.

[0036] 2. Although the in-situ synthesis method can effectively improve the dispersibility of zinc oxide, improper control of the reaction conditions and post-treatment during the in-situ synthesis may also lead to agglomeration between particles, making the dispersion effect of zinc oxide still insufficient.

[0037] Polystyrene can be used as a carrier to adsorb or embed zinc oxide into its matrix, so that a protective layer is formed on the surface of zinc oxide, allowing zinc oxide to be dispersed in the polystyrene matrix. Polystyrene can also reduce the interfacial tension between zinc oxide and the solvent, making zinc oxide more easily wetted. The improvement in wettability is conducive to better dispersion of zinc oxide in the solvent. Therefore, polystyrene is added to the zinc oxide precursor solution to improve the dispersibility of zinc oxide.

[0038] 3. Since polystyrene and zinc oxide are added separately, there is a situation where the reaction between polystyrene and zinc oxide is hindered by other components, which makes it impossible for polystyrene to disperse and modify zinc oxide, which in turn leads to insufficient anti-ultraviolet performance of zinc oxide.

[0039] Compared with adding polystyrene and zinc oxide separately, pre-connecting polystyrene with zinc oxide by grafting effectively reduces the possibility of obstruction between polystyrene and zinc oxide by other components, thereby promoting better dispersion of zinc oxide, and ultimately resulting in better UV resistance of the polyurethane composite material. DETAILED DESCRIPTION

[0040] The present application is further described in detail below in conjunction with Examples 1-7 and Comparative Examples 1-2.

[0041] raw material

[0042] Zinc acetate CAS: 557-34-6; Vinyl triethoxysilane CAS: 78-08-0; Anhydrous ethanol CAS: 64-17-5; Styrene CAS: 100-42-5; Initiator BPO CAS: 94-36-0; Toluene CAS: 108-88-3; Allyl glycidyl ether CAS: 106-92-3; Platinum tetrachloride CAS: 13454-96-1; Isopropyl ketone CAS: 67-63-0; Heptamethyl trisiloxane CAS: 1873-88-7; Diethylene glycol CAS: 111-46-6; Boron trifluoride ether CAS: 109-63-7; Propylene oxide CAS : 75-56-9; polypropylene carbonate diol CAS: 24937-06-2; dimer acid diisocyanate CAS: 68239-06-5; dibutyltin dilaurate CAS: 77-58-7; acetone CAS: 67-64-1; tetrahydrofuran CAS: 109-99-9; isophorone diamine CAS: 2855-13-2; polyetheramine D-230 CAS: 9046-10-0.

[0043] Example

[0044] Example 1

[0045] An anti-ultraviolet polyurethane composite material comprises the following raw materials: 2.5 mol dimer acid diisocyanate, 0.8 mol polypropylene carbonate diol, 0.25 mol siloxane modified polyether, 1.2 mol isophorone diamine, 1.2 mol polyetheramine D-230 and 0.375 mol / L zinc oxide precursor solution.

[0046] Specifically, the preparation method of the UV-resistant polyurethane composite material comprises the following steps:

[0047] S1: Weigh 0.6 mol of allyl glycidyl ether into a four-necked flask, add an isopropanol solution containing 0.004 mol of a reaction catalyst, platinum tetrachloride, heat to 90°C, stir for 0.5 h to complete activation, slowly dropwise add 0.15 mol of heptamethyltrisiloxane and react for 4 h, remove impurities, and obtain siloxane-modified glycidyl ether;

[0048] S2: Add siloxane-modified glycidyl ether, 0.5 mol of initiator diethylene glycol and 0.005 mol of catalyst boron trifluoride·ethyl ether into a flask, heat to 60°C and react for 0.5 h to complete activation, cool to 5°C in an ice-water bath, slowly add 2.5 mol of propylene oxide dropwise into the flask, stir and react for 5 h to obtain siloxane-modified polyether;

[0049] S3: Weigh 0.8 mol of a mixture of polypropylene carbonate diol and 0.25 mol of a siloxane-modified polyether and add it to a four-necked flask, vacuum dehydrate at 120-130° C. for 2 h, then cool to 80° C., add 3 mol of dimer acid diisocyanate and 0.19 mol of a catalyst dibutyltin dilaurate, and react for 3 h to obtain a polyurethane prepolymer;

[0050] S4: Add a mixture of 0.065 mol of ethanol and 2.24 mol of acetone to the polyurethane prepolymer, add 0.375 mol of zinc oxide precursor solution and emulsifier sodium ethylenediamine sulfonate, continue to stir at 55°C for 0.75h for emulsification, then evaporate the acetone at 94°C at normal pressure until no odor is detected, cool to room temperature, add water to dilute to the required concentration, and obtain an in-situ synthesized zinc oxide polyurethane solution;

[0051] Preparation of zinc oxide precursor solution: weigh 1 mol of zinc acetate and put it into deionized water, filter it after stirring, put the filtered zinc acetate into a vacuum drying oven to dry, add the vacuum-dried zinc acetate into an anhydrous ethanol solution containing 1.2 mol of vinyl triethoxysilane, wash it with anhydrous ethanol after the reaction is completed, and then wash away the anhydrous ethanol with deionized water to obtain a modified vinyl zinc salt solution;

[0052] Add 1.2 mol of styrene and 0.01 mol of initiator BPO into a polymerization bottle, then add vinyl zinc salt solution, seal the bottle mouth after vacuuming and nitrogen replacement, place the polymerization bottle in an oil bath, stir and react at 60°C for 4-6 hours, add deionized water after the reaction, and ultrasonically dissolve to obtain a zinc oxide precursor solution.

[0053] S5: Then, tetrahydrofuran was added to dissolve, cooled to 10°C with ice water, and 1.2 mol of isophorone diamine and 1.2 mol of polyetheramine D-230 were slowly added dropwise. After the addition was completed, the mixture was stirred and reacted for 3 hours;

[0054] S6: Pour the zinc oxide polyurethane solution into a polytetrafluoroethylene mold and place it in a fume hood to air dry to obtain a zinc oxide polyurethane elastomer.

[0055] Example 2-3

[0056] The difference from Example 1 is that the added amounts of the components of the UV-resistant polyurethane composite material are different, as shown in Table 1.

[0057] Table 1 Addition amount of each component of the UV-resistant polyurethane composite material in Examples 1-3

[0058] Example 1 Example 2 Example 3 Dimer Acid Diisocyanate 2.5mol 2mol 3mol Polypropylene carbonate glycol 0.8mol 1mol 0.6mol Siloxane modified polyether 0.25mol 0.1mol 0.4mol Isophorone diamine 1.2mol 2mol 0.4mol Polyetheramine D-230 1.2mol 0.4mol 2mol Zinc oxide precursor solution 0.375mol / L 0.5mol / L 0.25mol / L

[0059] Example 4

[0060] The difference from Example 1 is that the vinyl zinc salt solution is replaced by a zinc salt solution;

[0061] Preparation of zinc salt solution:

[0062] Zinc acetate is put into deionized water, and after stirring, it is filtered, and the filtered zinc acetate is put into a vacuum drying oven for drying. The vacuum-dried zinc acetate is added into anhydrous ethanol, and after the reaction is completed, it is washed with anhydrous ethanol, and then the anhydrous ethanol is washed away with deionized water.

[0063] Example 5

[0064] The difference from Example 4 is that no styrene is added.

[0065] Embodiment 6-7

[0066] The difference from Example 1 is that the addition amount of each component in the zinc oxide precursor solution is different, as shown in Table 2.

[0067] Table 2 Addition amount of each component in the zinc oxide precursor solution in Example 1 and Examples 6-7

[0068] Example 1 Example 6 Example 7 Zinc acetate 1mol 0.9mol 1.1mol Vinyltriethoxysilane 1.2mol 1.3mol 1.1mol Styrene 1.2mol 1.1mol 1.3mol Initiator BPO 0.01mol 0.009mol 0.02mol

[0069] Comparative Example

[0070] Comparative Example 1

[0071] The difference from Example 1 is that no zinc oxide precursor solution is added.

[0072] Comparative Example 2

[0073] The difference from Example 1 is that the zinc oxide precursor solution is replaced with the same added amount of zinc oxide.

[0074] Performance testing

[0075] Detection Methods

[0076] 1. Anti-ultraviolet performance test

[0077] Three samples were taken out from Examples 1-7 and Comparative Examples 1-2, respectively, and isophorone diamine and polyetheramine D-230 were added. After stirring, they were coated on a 76mm×26mm×0.5mm glass slide using a 10μm-50μm QXG wire rod coater, and dried at room temperature for 7 days to prepare coating samples with a dry film thickness of 10±2μm. Subsequently, the light transmittance of different coating samples at 300nm, 360nm and 560nm was tested using a UV-265 ultraviolet spectrophotometer and the average value was taken, wherein the ultraviolet shielding rate = 1-transmittance.

[0078] The test data are shown in Table 3.

[0079] Table 3 Anti-ultraviolet performance test table of Examples 1-7 and Comparative Examples 1-2

[0080]

[0081]

[0082] 2. Antibacterial performance test

[0083] Three samples were taken from Examples 1-7 and Comparative Examples 1-2, respectively, and the antibacterial performance was tested with reference to GB / T 21866-2008 "Determination of antibacterial properties and antibacterial effects of antibacterial coatings (paint films)", and then the antibacterial rates were obtained and the average value was taken.

[0084] The test data are shown in Table 4.

[0085]

[0086]

[0087] Referring to Example 1 and Comparative Examples 1-2 and in combination with Tables 3 and 4, it can be seen that, relative to Comparative Example 1, although the light transmittance of Comparative Example 1 and Comparative Example 2 at 560nm is not much different, relative to Comparative Example 1, the light transmittance of Comparative Example 2 at 300nm and 360nm is significantly reduced. Therefore, the ultraviolet shielding rate of Comparative Example 2 is significantly improved, and the antibacterial rate is also significantly improved. This shows that, relative to conventional self-healing polyurethane coatings, the addition of zinc oxide can effectively improve the anti-ultraviolet and antibacterial properties of the self-healing polyurethane coating.

[0088] Referring to Examples 1-3 and in combination with Tables 3 and 4, it can be seen that, relative to Example 1, the light transmittance of Examples 2 and 3 is increased, and thus the UV shielding rate and the antibacterial rate are decreased. This indicates that the amount of each component added also affects the UV resistance and antibacterial properties of the self-healing polyurethane coating.

[0089] With reference to Example 1 and Examples 4-5 and in combination with Table 3 and Table 4, it can be seen that, relative to Example 1, the light transmittance of Example 4 is increased, that is, the ultraviolet shielding rate of Example 4 is decreased, and the antibacterial rate of Example 4 is also decreased, while the light transmittance of Example 5 is further increased relative to Example 4, that is, the ultraviolet shielding rate of Example 5 is further decreased relative to Example 4, and the antibacterial rate of Example 5 is also further decreased, which indicates that the addition of styrene can improve the anti-ultraviolet and antibacterial properties of the self-healing polyurethane coating.

[0090] With reference to Example 1 and Comparative Example 2 and in combination with Tables 3 and 4, it can be seen that, relative to Example 1, the light transmittance of Comparative Example 2 at 300nm and 360nm is significantly increased, so the ultraviolet shielding rate and the antibacterial rate are significantly decreased. This shows that, relative to the use of a zinc oxide precursor solution, the use of zinc oxide directly in situ synthesized with a polyurethane prepolymer will result in a significant deterioration in the anti-ultraviolet performance and antibacterial performance of the self-healing polyurethane coating.

[0091] The reason is that conventional zinc oxide has high surface energy, irregular particle shape, surface charge and polarity, resulting in strong interaction between particles, easy aggregation to form agglomerates, and weak interaction in non-polar or low-grade media, which leads to poor uniform dispersion of zinc oxide. Therefore, when zinc oxide is directly added to the polyurethane prepolymer in Comparative Example 2, due to the insufficient dispersion performance of zinc oxide, the anti-ultraviolet and antibacterial properties of the sample in Comparative Example 2 are poorer than those in Example 1. Since the zinc oxide precursor solution in Example 1 is obtained by modifying zinc acetate to obtain a vinyl zinc salt solution, and then grafting the vinyl zinc salt solution with polystyrene, the ability of zinc oxide to be uniformly dispersed can be improved, thereby improving the anti-ultraviolet and antibacterial properties of the polyurethane coating;

[0092] However, by replacing the vinyl zinc salt solution with a zinc salt solution, the zinc salt solution cannot be grafted with the polystyrene, and the zinc salt solution can only be physically mixed with the polystyrene. The dispersibility of the zinc oxide precursor solution obtained after the physical mixing is lower than the dispersibility of the zinc oxide precursor solution in Example 1. In Example 5, styrene is no longer added, so that the vinyl zinc salt solution cannot be grafted with styrene, which will affect the dispersibility of the zinc oxide precursor solution to a certain extent, thereby causing the anti-ultraviolet performance and antibacterial performance of the polyurethane coating to be reduced.

[0093] With reference to Example 1 and Examples 6-7 and in combination with Table 3 and Table 4, it can be seen that, relative to Example 1, the light transmittance of Example 6 and Example 7 is increased, that is, the ultraviolet shielding rate of Example 6 and Example 7 is decreased, and the antibacterial rate of Example 6 and Example 7 is also decreased, which shows that the addition amount of each component in the zinc oxide precursor solution also affects the anti-ultraviolet performance and antibacterial performance of the self-healing polyurethane coating.

[0094] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-ultraviolet polyurethane composite material, characterized in that: The method comprises the following raw materials: 2-3 mol dimer acid diisocyanate, 0.6-1 mol polypropylene carbonate diol, 0.1-0.4 mol siloxane modified polyether, 0.4-2 mol isophorone diamine, 0.4-2 mol polyetheramine D-230 and 0.25-0.5 mol / L zinc oxide precursor solution. The zinc oxide precursor solution is used for in-situ synthesis of zinc oxide polyurethane.

2. The UV-resistant polyurethane composite material according to claim 1, characterized in that: The zinc oxide precursor solution is prepared by using zinc acetate as a zinc source.

3. The UV-resistant polyurethane composite material according to claim 2, characterized in that: The zinc oxide precursor solution contains polystyrene.

4. The UV-resistant polyurethane composite material according to claim 3, characterized in that: The zinc oxide precursor solution is a polystyrene grafted vinyl zinc salt solution.

5. The anti-ultraviolet polyurethane composite material according to claim 4, characterized in that: The preparation method of the vinyl zinc salt solution comprises the following steps: weighing zinc acetate and putting it into deionized water, filtering the zinc acetate after stirring, drying the filtered zinc acetate in a vacuum drying oven, adding the vacuum-dried zinc acetate into an anhydrous ethanol solution containing vinyl triethoxysilane, washing with anhydrous ethanol after the reaction is completed, and then washing away the anhydrous ethanol with deionized water to obtain a modified vinyl zinc salt solution.

6. The anti-ultraviolet polyurethane composite material according to claim 5, characterized in that: The preparation method of the zinc oxide precursor solution comprises the following steps: adding styrene and initiator BPO into a polymerization bottle, then adding a vinyl zinc salt solution, sealing the bottle mouth after vacuuming and nitrogen replacement, placing the polymerization bottle in an oil bath, stirring and reacting at 60° C. for 4-6 hours, adding deionized water after the reaction, and ultrasonically dissolving to obtain the zinc oxide precursor solution.

7. The anti-ultraviolet polyurethane composite material according to claim 6, characterized in that: The method comprises the following raw materials: 0.9-1.1 mol zinc acetate, 1.1-1.3 mol vinyl triethoxy silane, 1.1-1.3 mol styrene and 0.009-0.02 mol initiator BPO.

8. The method for preparing an anti-ultraviolet polyurethane composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: Weigh allyl glycidyl ether and place it in a four-necked flask, add isopropanol solution of platinum tetrachloride as a reaction catalyst, heat to 90°C, stir for 0.5h to complete activation, slowly drop heptamethyltrisiloxane and react for 4h, remove impurities, and obtain siloxane-modified glycidyl ether; S2: Add siloxane-modified glycidyl ether, initiator diethylene glycol and catalyst boron trifluoride·ethyl ether into a flask, heat to 60°C and react for 0.5h to complete activation, cool to 5°C in an ice-water bath, slowly add propylene oxide dropwise into the flask, stir and react for 5h to obtain siloxane-modified polyether; S3: Weigh a mixture of polypropylene carbonate diol and a small amount of siloxane-modified polyether and add it to a four-necked flask, vacuum dehydrate at 120-130° C. for 2 h, then cool to 80° C., add dimer acid diisocyanate and catalyst dibutyltin dilaurate, and react for 3 h to obtain a polyurethane prepolymer; S4: Add a mixture of 2-4 parts by mass of ethanol and 120-140 parts by mass of acetone to the polyurethane prepolymer, add the zinc oxide precursor solution and the emulsifier, continue to stir at 50-60°C for 0.5-1h for emulsification, then evaporate the acetone at 94°C under normal pressure until no odor is detected, cool to room temperature, add water to dilute to the required concentration, and obtain an in-situ synthesized zinc oxide polyurethane solution; S5: Then, tetrahydrofuran was added to dissolve, cooled to 10°C with ice water, and isophorone diamine and polyetheramine D-230 were slowly added dropwise. After the addition was completed, the mixture was stirred and reacted for 3 hours; S6: Pour the zinc oxide polyurethane solution into a polytetrafluoroethylene mold and place it in a fume hood to air dry to obtain a zinc oxide polyurethane elastomer.