High-voltage electrolyte additive as well as preparation method and application thereof
The zwitterionic polymer electrolyte additive obtained by adding branched polyethyleneimine to the aqueous electrolyte reaction with 1,3-propanesulfonolide has been destroyed, and the low conductivity of the aqueous electrolyte is solved. The problem of viscosity increases the working voltage and energy density of lithium-ion batteries and supercapacitors, and reduces the preparation cost.
Patent Information
- Application Number
- CN202411181212.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The low ionic conductivity and excessive viscosity of existing aqueous electrolytes limit the working voltage and energy density of lithium-ion batteries and supercapacitors, and the preparation cost is high.
Zwitterionic polymer electrolyte additives are prepared by reacting branched polyethyleneimine with 1,3-propanesulfonolide, and added to the aqueous electrolyte to destroy the hydrogen bond network between water molecules and improve the electrochemical stability of the electrolyte. Window and ionic conductivity.
It significantly improves the electrochemical stability window and ionic conductivity of the aqueous electrolyte, extends the working voltage and energy density of the energy storage device, reduces the preparation cost, and improves the fluidity of the electrolyte.
Smart Images

Figure CN119081106A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage, and in particular relates to a high-voltage electrolyte additive and a preparation method and application thereof. Background Art
[0002] At present, electrochemical energy storage is one of the simplest and most efficient ways of various existing energy storage methods. Electrochemical energy storage devices and equipment include secondary batteries, electrochemical supercapacitors or an organic combination of the two. Among them, lithium-ion batteries have developed rapidly due to their outstanding advantages such as long cycle stability, high energy density, and low self-discharge rate. During the charge-discharge process of lithium-ion batteries, lithium ions can be reversibly embedded in and extracted from the electrode active material, thereby completing the reversible conversion of electrical energy and chemical energy, and the crystal structure of the electrode material is not destroyed during the charge-discharge process. Supercapacitors, also known as electrochemical capacitors, are considered to be excellent candidates for the next generation of energy storage systems due to their fast charge and discharge rates, high power density, long cycle life, good safety and environmental friendliness. The energy storage mechanism of supercapacitors can be mainly divided into electrochemical double-layer capacitors and pseudocapacitors. The charge storage mechanism of electrochemical double-layer capacitors is the electrostatic interaction at the interface between electrodes and electrolytes, while pseudocapacitors use fast and reversible Faradaic oxidation-reduction reactions to store charge.
[0003] Electrolyte is a key material for electrochemical energy storage devices including lithium-ion batteries and supercapacitors, and its performance has an important influence on the internal resistance, life, rate performance, etc. of the device. Although the currently commonly used organic electrolytes have good salt dissolving ability and high electrochemical stability window, their toxicity and flammability cause serious safety hazards in the use of such energy storage devices. Aqueous electrolytes have the advantages of low cost and high safety performance, which can eliminate the safety hazards brought by organic electrolytes. At the same time, the ionic conductivity of aqueous electrolytes is usually high, which is conducive to the high rate performance of electrochemical energy storage devices. However, the electrochemical stability window of conventional aqueous electrolytes is narrow. Since the energy density of electrochemical devices is proportional to the operating voltage, the energy density of electrochemical devices can be increased by increasing the operating voltage value, which is especially effective for double-layer supercapacitors. Therefore, one of the keys to increasing the operating voltage of aqueous energy storage devices is to obtain aqueous electrolytes with a wide electrochemical stability window.
[0004] One of the common methods to broaden the electrochemical window of aqueous electrolytes is to prepare an aqueous solution of high-concentration salt, that is, a "water-in-salt" electrolyte. However, the preparation of water-in-salt electrolytes requires the use of a large amount of expensive lithium salts such as lithium trifluorosulfonyl imide, which results in a very high preparation cost of the aqueous electrolyte. In addition, the viscosity of water-in-salt electrolytes is relatively high, and salting out often occurs. In addition, some studies have improved the electrochemical stability window of aqueous electrolytes by adding additives such as small organic molecules or high molecular weight polymers to the electrolyte solution, and utilizing the strong interaction between these additive molecules and water molecules to destroy the hydrogen bond network between water molecules. However, the amount of these additives added is generally very large, which makes the electrolyte system essentially deviate from the aqueous electrolyte system, and also leads to negative problems such as low ionic conductivity and excessive viscosity of the electrolyte.
[0005] Therefore, it is necessary to develop a new type of high-voltage electrolyte additive and aqueous electrolyte system to increase the working voltage of aqueous energy storage devices and improve existing problems such as low ion conductivity and excessive viscosity. Summary of the invention
[0006] The present invention aims to provide a high-voltage electrolyte additive and a preparation method and application thereof. The zwitterionic polymer electrolyte additive is prepared by reacting branched polyethyleneimine with 1,3-propane sultone, which effectively improves the problems of low ion conductivity and high viscosity of aqueous electrolytes and increases the operating voltage of energy storage devices.
[0007] In a first aspect, the present invention provides a method for preparing a high-voltage electrolyte additive, comprising the following steps:
[0008] In solvent 1, under heating conditions, branched polyethyleneimine reacts with 1,3-propane sultone to obtain a reaction mixture;
[0009] The reaction mixture is added into a second solvent for precipitation, and the precipitation is dried to obtain the electrolyte additive.
[0010] Optionally, solvent one includes any one of trifluoroethanol and hexafluoroisopropanol.
[0011] Optionally, the second solvent includes any one of tetrahydrofuran, ethanol, acetone, acetonitrile and dioxane.
[0012] Optionally, the volume ratio of solvent one to solvent two is 1:10.
[0013] Optionally, the branched polyethyleneimine includes any one of branched polyethyleneimines with a molecular weight of 300, 600, and 900.
[0014] Optionally, when the molecular weight of the branched polyethyleneimine is 600, the structural formula of the prepared electrolyte additive is as shown in Formula I:
[0015]
[0016] Optionally, the heating condition is 30-70° C., and the reaction time is 12-96 hours.
[0017] Optionally, the mass ratio of the branched polyethyleneimine to the 1,3-propane sultone is 1:(1-10).
[0018] In a second aspect, the present invention provides an aqueous electrolyte prepared using a high-voltage electrolyte additive.
[0019] Optionally, the aqueous electrolyte includes the high-voltage electrolyte additive, water, and a soluble salt.
[0020] Optionally, the soluble salt includes at least one of lithium sulfate, lithium hydroxide, lithium nitrate, lithium acetate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), sodium chloride, sodium sulfate, sodium perchlorate, etc.
[0021] Optionally, the mass ratio of the high-voltage electrolyte additive to water is (1-9):(1-9).
[0022] Optionally, the concentration of soluble salt in the aqueous electrolyte is 0.5-21m (mol / kg).
[0023] Optionally, at 25-30° C., the electrochemical stability window of the aqueous electrolyte is 2.5-3.5V.
[0024] Optionally, at 25-30° C., the ionic conductivity of the aqueous electrolyte is 0.5-10 mS / cm.
[0025] In a third aspect, the present invention provides an application of an aqueous electrolyte in the preparation of an electrochemical energy storage device, characterized in that the application includes an aqueous secondary battery, an aqueous electrochemical supercapacitor, and an aqueous hybrid capacitor.
[0026] The beneficial effects of the present invention include:
[0027] (1) The preparation method of high-voltage electrolyte addition provided by the present invention has low cost, stable output, and good application prospects;
[0028] (2) The high-voltage electrolyte additive provided by the present invention introduces a branched or hyperbranched zwitterionic polymer as an additive into an aqueous electrolyte. Since the polymer molecules with a branched or hyperbranched structure have a compact structure similar to a sphere, a small hydrodynamic radius of gyration, and less molecular chain entanglement, the increase in relative molecular mass has little effect on the viscosity. In addition, the branched or hyperbranched polyethyleneimine raw material molecules have reactive functional groups, which can be modified to have zwitterionic groups and then added to the electrolyte as an additive to effectively control the viscosity of the electrolyte. The strong interaction between the zwitterionic groups in the polymer added to the electrolyte and the water molecules restrains the movement of the water molecules, destroys the hydrogen bond network between the water molecules, increases the decomposition voltage of the electrolyte, and increases the electrochemical stable voltage window of the aqueous electrolyte, thereby increasing the energy density of the energy storage device. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Cyclic voltammetry curves of supercapacitors assembled with the 2m-60%-600PESB electrolyte provided in Example 3 of the present invention in different operating voltage windows;
[0030] Figure 2 Cyclic voltammetry curves of supercapacitors assembled with the 2m-70%-600PESB electrolyte provided in Example 4 of the present invention in different operating voltage windows;
[0031] Figure 3 Cyclic voltammetry curves of a supercapacitor assembled with the 2m-60%-600PEI electrolyte provided in Comparative Example 1 of the present invention under different operating voltage windows;
[0032] Figure 4 The constant current charge-discharge curve of the supercapacitor assembled with the 2m-60%-600PESB electrolyte provided in Example 3 of the present invention in a 2.3V voltage window;
[0033] Figure 5 The constant current charge-discharge curve of the supercapacitor assembled with the 2m-70%-600PESB electrolyte provided in Example 4 of the present invention in a 2.5V voltage window;
[0034] Figure 6 The curve of the change of specific capacitance of the supercapacitor assembled with the 2m-60%-600PESB electrolyte provided in Example 3 of the present invention as a function of current density;
[0035] Figure 7 Energy density and power density curves of the supercapacitor assembled with the 2m-60%-600PESB electrolyte provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0036] The present invention will be further described through the following embodiments in conjunction with the accompanying drawings.
[0037] In a first aspect, an embodiment of the present invention provides a method for preparing a high-voltage electrolyte additive, comprising the following steps:
[0038] In solvent 1, under heating conditions, branched polyethyleneimine reacts with 1,3-propane sultone to obtain a reaction mixture;
[0039] The reaction mixture is added into a second solvent for precipitation, and the precipitation is dried to obtain the electrolyte additive.
[0040] In some embodiments, solvent one includes any one of trifluoroethanol and hexafluoroisopropanol.
[0041] In some embodiments, the second solvent includes any one of tetrahydrofuran, ethanol, acetone, acetonitrile, and dioxane.
[0042] In some embodiments, the volume ratio of solvent 1 to solvent 2 is 1:10.
[0043] In some embodiments, the branched polyethyleneimine comprises any one of branched polyethyleneimine with a molecular weight of 300, 600, and 900.
[0044] In some embodiments, when the molecular weight of the branched polyethyleneimine is 600, the structural formula of the prepared electrolyte additive is as shown in Formula I:
[0045]
[0046] In some embodiments, the heating condition is 30-70° C., and the reaction time is 12-96 hours.
[0047] In some embodiments, the mass ratio of the branched polyethyleneimine to the 1,3-propane sultone is 1:(1-10).
[0048] In a second aspect, an embodiment of the present invention provides an aqueous electrolyte prepared by using a high-voltage electrolyte additive.
[0049] In some embodiments, the aqueous electrolyte includes the high-voltage electrolyte additive, water, and a soluble salt.
[0050] In some embodiments, the soluble salt includes at least one of lithium sulfate, lithium hydroxide, lithium nitrate, lithium acetate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), sodium chloride, sodium sulfate, sodium perchlorate, etc.
[0051] Specifically, the mass ratio of the high-voltage electrolyte additive to water is (1-9):(1-9).
[0052] In some embodiments, the concentration of soluble salt in the aqueous electrolyte is 0.5-21m (mol / kg).
[0053] In some embodiments, at 25-30° C., the electrochemical stability window of the aqueous electrolyte is 2.5-3.5V.
[0054] In some embodiments, at 25-30° C., the ionic conductivity of the aqueous electrolyte is 0.5-10 mS / cm.
[0055] In a third aspect, an embodiment of the present invention provides an application of an aqueous electrolyte in the preparation of an electrochemical energy storage device, characterized in that the application includes an aqueous secondary battery, an aqueous electrochemical supercapacitor, and an aqueous hybrid capacitor.
[0056] Example 1
[0057] Embodiment 1 of the present invention provides a method for preparing a high-voltage electrolyte additive, comprising the following steps:
[0058] 3 g of branched polyethyleneimine (PEI) with a relative molecular mass of 600 was placed in a round-bottom flask, 25 mL of trifluoroethanol was added, and 12.3 g of 1,3-propane sultone was added dropwise to the round-bottom flask; the mixture was heated to 40° C. in an oil bath and stirred for 72 h to obtain a reaction mixture;
[0059] The reaction mixture was added dropwise to 250 mL of tetrahydrofuran through a dropping funnel. After the addition was completed, the white precipitate in the tetrahydrofuran was taken out and dried in a vacuum drying oven at 60° C. for 12 h to obtain a branched zwitterionic polymer additive, namely, a high-voltage electrolyte additive 600PESB, with a structural formula as shown in Formula I.
[0060]
[0061] Example 2
[0062] Embodiment 2 of the present invention provides a method for preparing a high-voltage electrolyte additive, which is different from Embodiment 1 in that a branched PEI with a relative molecular mass of 300 is used for preparation, and other conditions and steps remain the same to obtain a high-voltage electrolyte additive 300PESB.
[0063] Example 3
[0064] Embodiment 3 of the present invention provides a method for preparing an aqueous electrolyte, comprising the following steps:
[0065] 2.8 g (0.01 mol) of lithium bis(trifluoromethanesulfonyl)imide electrolyte was dissolved in 2 g of deionized water, and 3 g of the high-voltage electrolyte additive 600PESB prepared in Example 1 was added; the mass ratio of water to additive was 4:6, the electrolyte concentration was 2 m, and the aqueous electrolyte 2m-60%-600PESB was prepared.
[0066] Example 4
[0067] Embodiment 4 of the present invention provides a method for preparing an aqueous electrolyte, which is different from Embodiment 3 in that the mass ratio of water to additive is 3:7, and other conditions and steps remain the same, to prepare an aqueous electrolyte 2m-70%-600PESB.
[0068] Example 5
[0069] Embodiment 5 of the present invention provides a method for preparing an aqueous electrolyte, which is different from Embodiment 3 in that the mass ratio of water to additive is 5:5, and other conditions and steps remain the same, to prepare an aqueous electrolyte 2m-50%-600PESB.
[0070] Example 6
[0071] Embodiment 6 of the present invention provides a method for preparing an aqueous electrolyte, which is different from Embodiment 3 in that the aqueous electrolyte is prepared using the high-voltage electrolyte additive 300PESB prepared in Embodiment 2; other conditions and steps remain the same to prepare an aqueous electrolyte 2m-60%-300PESB.
[0072] Example 7
[0073] Embodiment 7 of the present invention provides a method for preparing an aqueous electrolyte, which is different from Embodiment 3 in that the aqueous electrolyte is prepared using the high-voltage electrolyte additive 300PESB prepared in Embodiment 2; the mass ratio of water to the additive is 3:7; other conditions and steps remain consistent, and an aqueous electrolyte 2m-70%-300PESB is obtained.
[0074] Comparative Example 1
[0075] Comparative Example 1 of the present invention provides a method for preparing an aqueous electrolyte, which is different from Example 3 in that 600PEI is used as an additive to prepare an aqueous electrolyte 2m-60%-600PEI.
[0076] Performance Verification
[0077] 1. Determination of ionic conductivity of aqueous electrolyte
[0078] The ionic conductivity of the aqueous electrolyte was detected using electrochemical impedance spectroscopy, and the detection results of Examples 3-7 and Comparative Example 1 are shown in Table 1.
[0079] Table 1 Ionic conductivity test results
[0080]
[0081] Referring to Table 1, the ionic conductivity of the aqueous electrolytes prepared in Examples 3-7 of the present invention using PESB branched zwitterionic polymer as an electrolyte additive is higher than that of Comparative Example 1, which proves that the present invention can significantly improve the ionic conductivity of the aqueous electrolyte by using PESB as an additive.
[0082] 2. Performance testing of supercapacitors assembled with aqueous electrolyte
[0083] The aqueous electrolytes prepared in Example 3, Example 4 and Comparative Example 1 were respectively assembled into aqueous supercapacitors to compare the high voltage performance, including the following steps:
[0084] Activated carbon (AC), acetylene black, and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1 were dispersed in N-methylpyrrolidone (NMP) to prepare a uniform dispersion slurry;
[0085] The dispersion slurry was coated on titanium foil and dried under vacuum at 80 °C for 12 h to obtain an AC electrode. The loading amount of AC active material on the electrode was about 2.5 mg / cm 2 ;
[0086] A symmetrical capacitor is assembled using AC electrodes as positive and negative electrodes, the diaphragm is a Whatman glass fiber diaphragm, and the aqueous electrolytes are the aqueous electrolytes prepared in Example 3, Example 4, and Comparative Example 1 respectively;
[0087] The working voltage of three aqueous supercapacitors was detected by cyclic voltammetry, and the cyclic voltammetry curves were obtained. Figure 1-3 As shown;
[0088] The constant current charge-discharge curves of the supercapacitors prepared by the aqueous electrolytes of Examples 3 and 4 were tested by the constant current charge-discharge method. The results are as follows: Figure 4 , Figure 5 As shown;
[0089] See also Figure 1-3 In Examples 3 and 4, the working voltage of the supercapacitor assembled with the aqueous electrolyte solution adding 600 PESB of the high-voltage electrolyte additive can reach 2.5V, while in Comparative Example 1, which uses PEI alone as an additive, the working voltage of the assembled supercapacitor is lower than 2V;
[0090] See also Figure 4 , Figure 5The constant current charge-discharge curves of the supercapacitor assembled with the aqueous electrolyte 2m-60%-600PESB in Example 3 under the working voltage conditions of 2.3V and 2.5V respectively show a nearly symmetrical isosceles triangle profile, indicating a typical double-layer capacitor behavior;
[0091] See also Figure 6 , Figure 7 The current density and specific capacitance relationship curves and the power density and energy density relationship curves of the supercapacitor assembled with the aqueous electrolyte 2m-60%-600PESB in Example 3 were calculated by constant current charge and discharge curves. It can be seen that the assembled supercapacitor has very good rate performance and high energy density.
[0092] In summary, the addition of PESB significantly increases the operating voltage of the supercapacitor. This is because the branched zwitterionic polymer PESB is added as an additive to the aqueous electrolyte, which can destroy the hydrogen bond network between water molecules through strong interaction with water, increase the decomposition voltage of water molecules, and thus increase the operating voltage of the electrolyte in the device; therefore, the aqueous electrolyte prepared from the high-voltage electrolyte provided by the present invention can increase the operating voltage of the supercapacitor.
[0093] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing a high-voltage electrolyte additive, It is characterized in that The following steps are involved: In solvent 1, under heating conditions, branched polyethyleneimine reacts with 1,3-propane sultone to obtain a reaction mixture; The reaction mixture is added into a second solvent for precipitation, and the precipitation is dried to obtain the electrolyte additive.
2. The preparation method according to claim 1, It is characterized in that The solvent 1 includes any one of trifluoroethanol and hexafluoroisopropanol; the solvent 2 includes any one of tetrahydrofuran, ethanol, acetone, acetonitrile and dioxane.
3. The preparation method according to claim 1, It is characterized in that The mass ratio of the branched polyethyleneimine to the 1,3-propane sultone is 1:(1-10).
4. The preparation method according to claim 1, It is characterized in that The branched polyethyleneimine includes any one of a branched polyethyleneimine with a molecular weight of 300 and a branched polyethyleneimine with a molecular weight of 600; Wherein, when the molecular weight of the branched polyethyleneimine is 600, the structural formula of the prepared electrolyte additive is as shown in Formula I:
5. An aqueous electrolyte prepared by the high-voltage electrolyte additive prepared by the preparation method according to any one of claims 1 to 4, It is characterized in that The aqueous electrolyte includes the high-voltage electrolyte additive, water, and soluble salt.
6. The aqueous electrolyte according to claim 5, It is characterized in that The soluble salt includes at least one of lithium sulfate, lithium hydroxide, lithium nitrate, lithium acetate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), sodium chloride, sodium sulfate, sodium perchlorate, and the like.
7. The aqueous electrolyte according to claim 5, It is characterized in that The mass ratio of the high-voltage electrolyte additive to water is (1-9):(1-9).
8. The aqueous electrolyte according to claim 5, It is characterized in that The concentration of soluble salts in the aqueous electrolyte is 0.5-21m.
9. Use of the aqueous electrolyte according to any one of claims 5 to 8 in the preparation of an electrochemical energy storage device, It is characterized in that The applications include aqueous secondary batteries, aqueous electrochemical supercapacitors, and aqueous hybrid capacitors.
Citation Information
Patent Citations
Polyelectrolyte as well as preparation method and application thereof
CN111154098A
Sulfonated polyethyleneimine and nanofiltration membrane, and preparation methods thereof
CN111187413A
Electrode interface layer material, zwitterionic polymer and organic photovoltaic element.
CN112390947A
Anti-pollution protective layer of reverse osmosis membrane and preparation method of anti-pollution protective layer
CN118105858A
Plating solution
CN118265814A