Polyvinyl alcohol-based hydrogel with low hysteresis, fatigue resistance and high thermoelectricity and preparation method of polyvinyl alcohol-based hydrogel
A polyvinyl alcohol-based hydrogel with sodium alginate and ferrocyanides forms a dense network structure, addressing mechanical instability and low thermoelectricity issues, enabling flexible and durable energy conversion.
Patent Information
- Application Number
- CN202411447183.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-06
AI Technical Summary
Current thermoelectric hydrogels exhibit poor mechanical stability and low thermoelectric performance, limiting their application in flexible electronics and low-grade thermal energy collection.
A polyvinyl alcohol-based hydrogel is prepared using sodium alginate with carboxyl carbonyl groups, potassium ferrocyanides as redox pairs, and NaCl as free ions, forming a dense open-pore network structure through freeze-thaw and Hofmeister effects, enhancing mechanical toughness and thermoelectricity.
The hydrogel achieves low hysteresis fatigue resistance and high thermoelectricity, maintaining stability under external forces and extending device life, suitable for flexible sensing and low-grade heat collection.
Smart Images

Figure CN119081159A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-hysteresis fatigue-resistant and high-thermoelectric polyvinyl alcohol-based hydrogel and a preparation method thereof, belonging to the field of polymer thermoelectric hydrogel preparation and application thereof in energy and electronic technology. Background Art
[0002] Low-grade waste heat generated by industry or natural resources is collected through thermoelectric technology. The converted electricity can drive a series of low-power sensors, IoT devices and wearable devices, which can make a huge contribution to the upcoming energy crisis. According to the type of carrier, thermoelectric materials can be divided into electronic thermoelectric materials and ionic thermoelectric materials. The thermoelectric conversion effect of electronic thermoelectric materials is mainly based on the migration of electrons and holes under temperature difference, but its Seebeck coefficient (Se) is low. At the same time, its inherent stiffness cannot meet the requirements of flexible electronics, which limits its wide application. In contrast, based on the ion thermal diffusion effect (Soret effect) or the thermocurrent effect of oxidation / reduction pairs, the Se of ionic thermoelectric materials is two to three orders of magnitude higher than that of electronic thermoelectric materials, which has attracted more and more attention from researchers.
[0003] Polymer hydrogels with three-dimensional cross-linked network structures are ideal candidate materials for low-grade thermal energy collection and wearable electronics due to their high water content, flexibility and biocompatibility. Yang et al., Angew Chem Int Ed. 2016, 39, 12050-12053. Thermoelectric hydrogels were prepared by a one-pot method. The tensile strength of the hydrogels was about 0.11 MPa, the elongation at break was 220%, and the Se was about 1 mV·K -1 The thermoelectric hydrogel can be molded into different shapes for easy integration and packaging, opening up new prospects for thermal batteries and wearable functional electronic devices. Li et al., Energy Environ Mater. 2024, 2, e12547. Polyacrylic acid / xanthan gum / Bi2Se was prepared by in situ polymerization. 0.3 Te 2.7 Thermoelectric hydrogel, with a tensile strength of about 0.03 MPa and Se of -0.45 mV·K -1 , when the temperature difference is 40 K, its output voltage is -17.91 mV. This new thermoelectric hydrogel can effectively convert low-grade waste heat into electrical energy. However, the thermoelectric and mechanical properties of the thermoelectric hydrogels currently studied are still relatively low, which greatly limits their application in the field of low-grade thermal energy collection. In addition, polymer hydrogels with fatigue resistance and high thermoelectricity need further research and development to meet the application in energy and electronic technology fields such as wearable electronics, low-grade energy collection and security systems. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a polyvinyl alcohol-based hydrogel with low hysteresis, fatigue resistance and high thermoelectricity in view of the deficiencies of the prior art, so as to broaden the application scope of thermoelectric hydrogel. The method is characterized in that polyvinyl alcohol (PVA) with excellent elastic modulus is used as the matrix, sodium alginate (SA) containing a large number of carboxyl carbonyl groups is selected, and it is compounded with PVA, potassium ferrocyanide (K3Fe(CN)6) and potassium ferrocyanide (K4Fe(CN)6) are used as redox pairs, and NaCl is used as free ions, and PVA-based thermoelectric hydrogel (referred to as PSNF hydrogel) is prepared by freeze-thaw and Hofmeister effect research. There is a strong hydrogen bond interaction between PVA and SA molecular chains, forming a dense open-pore three-dimensional network structure, which gives PSNF hydrogel low hysteresis fatigue resistance; the open-pore network structure provides a channel for ion transmission, and due to the synergistic effect of the Soret effect and the thermocurrent effect, the thermoelectricity of the hydrogel is significantly improved. At the same time, the SA molecular chain rich in carboxyl carbonyl anions is Na + Providing a fast transmission channel, forming a potential difference at both ends of the electrode, further improving the thermoelectric properties of PSNF hydrogel.
[0005] The object of the present invention is achieved by the following technical measures, wherein the raw material fractions are all parts by weight unless otherwise specified.
[0006] A method for preparing a low-hysteresis fatigue-resistant and high-thermoelectric polyvinyl alcohol-based hydrogel comprises the following steps: 10 parts of PVA are added to 50-200 parts of water and dissolved at 95°C to obtain solution ①; 1-20 parts of SA are added to 20-100 parts of water and dissolved at 65°C to obtain solution ②; then 0.2-1 parts of NaCl, 0.2-1.5 parts of K3Fe(CN)6 and 0.26-1.95 parts of K4Fe(CN)6·3H2O (the two are in an equimolar ratio) are added to solution ②, and stirred to obtain solution ③; solution ① is cooled to 65°C, and then mixed with solution ③, and finally frozen at -20°C for 10-30 h, thawed for 4-20 h, and frozen and thawed 1-4 times to obtain PSNF hydrogel; Among them, the degree of polymerization of polyvinyl alcohol is 400-3000, and the degree of alcoholysis is 75-99%; The present invention has the following advantages
[0007] The present invention aims to prepare a method for preparing a polyvinyl alcohol-based hydrogel with low hysteresis fatigue resistance and high thermoelectricity in view of the shortcomings of the current thermoelectric hydrogel, which has poor mechanical stability and low thermoelectric performance, and to broaden the application range of thermoelectric hydrogel. PVA hydrogel with excellent mechanical toughness is used as the matrix, SA containing a large amount of carboxycarbonyl anions is introduced, potassium ferrocyanide (K3Fe(CN)6) and potassium ferrocyanide (K4Fe(CN)6) are used as redox pairs, and NaCl is used as free ions. PVA-based thermoelectric hydrogel (referred to as PSNF hydrogel) is prepared by freeze-thaw and Hofmeister effect research. During the freeze-thaw stage, certain hydrogen bonds and microcrystals are formed between PVA molecules and between PVA molecules and SA molecules, becoming physical crosslinking points, forming a dense open-pore three-dimensional network structure, giving PSNF hydrogel low hysteresis fatigue resistance; the gel open-pore network structure provides a channel for ion transmission. Due to the synergistic effect of the Soret effect and the thermocurrent effect, the thermoelectricity of the hydrogel is significantly improved. At the same time, the SA molecular chain rich in carboxycarbonyl anions is Na + Providing a fast transmission channel, forming an electric potential difference at both ends of the electrode, further improving the thermoelectric gel low hysteresis fatigue resistance of PSNF hydrogel, so that it can still maintain good stability under the action of external force and extend the service life of the device, and it can be used in applications such as flexible sensing, low-grade heat collection and security systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0009] Figure 1 Schematic diagram of the preparation of low hysteresis fatigue-resistant and high thermoelectric PSNF hydrogel.
[0010] Figure 2 Mechanical properties of hydrogel.
[0011] Figure 3 Application of thermoelectric properties of PSNF hydrogel. DETAILED DESCRIPTION
[0012] The present invention is described in detail below through examples. It is necessary to point out that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the contents of the present invention. Example 1
[0013] 5 g of PVA was added to 25 g of water and dissolved at 95°C to obtain solution ①; solution ① was frozen at -20°C for 16 h, thawed for 8 h, and frozen and thawed once to obtain PVA hydrogel. Example 2
[0014] 5 g PVA was added to 25 g water and dissolved at 95°C to obtain solution ①; 5 g SA was added to 25 g water and dissolved at 65°C to obtain solution ②; solution ① was cooled to 65°C, then mixed evenly with solution ②, and finally frozen at -20°C for 16 h, thawed for 8 h, and frozen and thawed once to obtain PVA / SA hydrogel. Example 3
[0015] 5 g PVA was added to 25 g water and dissolved at 95 °C to obtain solution ①. 0.5 g NaCl, 0.75 g K3Fe(CN)6 and 0.96 g K4Fe(CN)6·3H2O were added to 25 g water and stirred to obtain solution ②. Solution ① was cooled to 65 °C and then mixed with solution ②. Finally, the solution was frozen at -20 °C for 16 h, thawed for 8 h, and frozen and thawed once to obtain PNF hydrogel. Example 4
[0016] 5 g PVA was added to 25 g water and dissolved at 95 °C to obtain solution ①; 0.5 g SA was added to 25 g water and dissolved at 65 °C to obtain solution ②; then 0.5 g NaCl, 0.75 g K3Fe(CN)6 and 0.96 g K4Fe(CN)6·3H2O were added to solution ② and stirred to obtain solution ③; solution ① was cooled to 65 °C and then mixed with solution ③, and finally frozen at -20 °C for 16 h, thawed for 8 h, and frozen and thawed once to obtain PSNF hydrogel. Characterization of the hydrogel in this example:
[0017] Figure 2 The mechanical properties of the samples prepared in Examples 1-4 are as follows: Figure 2 As shown in (a, b), PSNF hydrogel has excellent comprehensive mechanical properties and a toughness of up to 1750 kJ·m -3 , the tensile strength, elongation and Young's modulus are 900 kPa, 450% and 220 kPa, respectively, which are much higher than those of PVA, PVA / SA and PNF hydrogels. Figure 2 c is the cyclic tensile stress-strain curve of PSNF hydrogel. The hydrogel underwent 20 cyclic stretching with a strain of 50%. The curves of each cycle almost overlapped, and the hysteresis circle was relatively small. Figure 2d is the continuous loading-unloading cyclic tensile curve of PSNF hydrogel under different strains (20-200%). Under large strain, the cyclic tensile curve still maintains a small hysteresis curve, indicating that the hysteresis of PSNF hydrogel is low and excellent fatigue resistance is achieved. Figure 2 As shown in Figure 5e, the dumbbell-shaped splines of PSNF hydrogel can be easily stretched to 280% of their original length without breaking and can immediately recover to their original length after stress release, and can also be bent and twisted and can immediately recover to their original state after stress release.
[0018] Crack propagation insensitivity is one of the important properties for evaluating the service life of hydrogels. Tensile tests were performed on unnotched and pre-notched PSNF hydrogels (notch depth 3 mm). Figure 2 As shown in f, the stress of the pre-notched specimen did not decrease significantly compared with that of the unnotched specimen. The fracture energy of the PSNF hydrogel was calculated to be 3.54 kJ·m -2 After stretching, the notch depth did not increase significantly compared to the initial depth ( Figure 2 g), indicating that PSNF is insensitive to crack growth. Figure 2 (h, i) are the puncture resistance tests of PVA, PVA / SA, PNF and PSNF hydrogels, and the puncture force (4.92 N) and puncture energy (59.34 mJ) of PSNF. The optical microscope images of PVA, PVA / SA, PNF and PSNF after puncture show that PVA has the largest puncture hole area and is severely damaged, the puncture hole area of PVA / SA and PNF decreases, and the puncture hole area of PSNF is the smallest (expanding from obvious cracks to only pinholes). The PSNF hydrogel was adhered to a plastic ring with a diameter of 25 mm, and the hydrogel was punctured with a flat-head screwdriver (diameter of 5 mm) under the condition of applying a weight of 200 g, as shown in Figure 2. Figure 2 As shown in Figure j, PVA, PVA / SA, and PNF hydrogels all suffered puncture failure, while PSNS hydrogel maintained its structural integrity and remained intact after the load was removed, indicating that PSNF hydrogel has excellent puncture resistance.
[0019] Figure 3 The application of the thermoelectric properties of PSNF hydrogel. After the PSNF hydrogel is integrated and connected to the LED light, when ΔT is about 17K, the PSNF hydrogel can light up 15 red bulbs (8.9 V) with the help of an amplifier (AD620). The LED light can be divided into six stages from the start to the end, corresponding to the PSNF hydrogel ΔV-time curve ( Figure 3a, b): The first stage is the non-working state (ΔT=0 K); in the second stage, after 18 seconds of ΔT (ΔT=12 K), the LED light is dim; in the third stage, the LED light gradually becomes brighter (ΔT=15 K); in the fourth stage, after 28 seconds of ΔT, the LED light reaches its brightest (ΔT=17 K). In the fifth stage (ΔT=17-2K), when the Peltier stops heating (that is, when the temperature difference gradually decreases), the LED light gradually dims; finally, in the sixth stage (ΔT=0 K), the LED light is completely off. The above experiments show that PSNF hydrogel can convert low-grade thermal energy in the environment into electrical energy, thereby realizing continuous power supply to external circuits. In addition, Figure 3 As shown in Figure c, we wore a flexible wristband consisting of 15 PSNF units on our arm, which can convert body temperature (36.5℃, ΔT=12 K) into electricity with the help of a voltage amplifier to successfully light up 15 LED bulbs, indicating the prospect of PSNF hydrogels in the application of wearable thermal energy harvesting devices.
[0020] In industrial production, too fast feed rate, incorrect feed ratio and feed sequence may lead to high reaction temperature. If cooling is not timely, it will lead to explosive polymerization, causing heavy casualties and property losses. Therefore, we proposed the concept of using PSNF hydrogel thermoelectric device for overheating alarm in industrial production. The concept diagram is shown in the figure. Figure 3 d. When high temperature causes ΔV to exceed a certain safety value, an alarm light will be triggered so that the safety officer can cool the reactor in time to avoid a larger accident. To evaluate the feasibility of the proposed concept, the output voltage of the original PSNF hydrogel and the control hydrogel (after 200 punctures) were continuously monitored under a cyclic temperature gradient (ΔT of 15 K, 40 K, and 70 K) to verify its excellent damage durability and ability to maintain accurate and stable voltage output in a long-term high temperature environment ( Figure 3 e). The results show that the output voltage of the PSNF hydrogel and the control hydrogel after 200 punctures increases with the increase of ΔT (15 K, 40 K and 70 K). After working for 5 cycles at 70 K (100°C), even if the structure is greatly damaged, ΔV can still be accurately detected and stably output, indicating that the PSNF hydrogel has excellent mechanical properties and stable output voltage, making it suitable for long-term overheating alarm equipment.
Claims
1. A method for preparing a low hysteresis fatigue-resistant and high thermoelectric polyvinyl alcohol-based hydrogel, characterized in that: The preparation method of the gel comprises the following steps: ① Dissolve polyvinyl alcohol in water at 95°C to obtain solution I; ② Dissolve sodium alginate in water at 65°C to obtain solution II; ③ Add NaCl, K3Fe(CN)6 and K4Fe(CN)6·3H2O to solution II and stir evenly to obtain solution III; ④ Cool solution I to 65°C, then mix evenly with solution III, and obtain PSNF hydrogel through freeze-thaw.
2. The method according to claim 1, characterized in that In the step ①, the mass fraction of polyvinyl alcohol in the solution is 5% to 20%, the degree of polymerization of polyvinyl alcohol is 400 to 3000, and the degree of alcoholysis is 75 to 99%.
3. The method according to claim 1, characterized in that: The mass fraction of sodium alginate in the solution in step ② is 5% to 20%.
4. The method according to claim 1, characterized in that In the step ③, the mass fraction of NaCl in the solution is 0.2%-5%, the mass fraction of K3Fe(CN)6 is 0.2%-7.5%, and the mass fraction of K4Fe(CN)6·3H2O is 0.26%-9.75%.
5. The method according to claim 1, characterized in that The freezing in step ④ is performed at -20±10°C for 10-30 h.
6. The method according to claim 1, characterized in that The thawing in step ④ is performed at room temperature for 4-20 hours.
7. The method according to claim 1, characterized in that The freezing-thawing process in step ④ is cycled 1-4 times.
8. A low hysteresis fatigue-resistant and high thermoelectric polyvinyl alcohol-based hydrogel prepared by the method according to any one of claims 1 to 7.
9. The low hysteresis fatigue-resistant and high thermoelectric polyvinyl alcohol-based hydrogel according to claim 8 is used in the fields of flexible sensing, low-grade heat collection and security systems.