Mixed ligand MOF polycrystalline film and preparation method and application thereof
The ligand exchange method in ZIF membranes adjusts pore sizes using ZIF-7 and ZIF-90 structures, addressing the limitations of existing ZIF membranes by achieving dense, defect-free gas separation with improved selectivity and stability.
Patent Information
- Application Number
- CN202411191138.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing ZIF membranes face challenges in achieving dense, defect-free structures with suitable pore sizes for high-throughput and high-selectivity gas separation, limiting their effectiveness in separating different gas mixtures.
A method involving a ligand exchange reaction to introduce mixed ligands into ZIF membranes, specifically using ZIF-7 and ZIF-90 structures to adjust pore sizes, combined with activation processes to create a mixed ligand MOF polycrystalline membrane.
The method results in a dense, defect-free membrane with precise control over pore size, enhancing gas separation selectivity and stability, enabling efficient separation of small and large gases.
Smart Images

Figure CN119081180A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of membrane materials, and in particular to a mixed ligand MOF polycrystalline membrane and a preparation method and application thereof. Background Art
[0002] Metal-organic framework (MOF) materials are a class of crystalline porous materials with periodic network structures formed by the self-assembly of inorganic metal centers (metal ions or metal clusters) and bridging organic ligands. Zeolitic imidazolate framework (ZIF) is a class of MOF materials composed of zinc ions and imidazole ligands. ZIF materials have high specific surface area and porosity, excellent thermal and chemical stability, and pore sizes close to the molecular dynamic diameter of gases, showing great potential as gas separation membrane materials. However, there are currently few ZIF membranes that exhibit excellent gas separation performance, and research has mainly focused on the design and preparation of ZIF-8 membranes and their application in propylene and propane separation. The main reasons are as follows: (1) It is difficult to obtain dense and defect-free ZIF membranes to achieve high-throughput and high-selectivity separation of gas mixtures; (2) It is difficult to find ZIF materials with suitable pore sizes and easy preparation for specific gas mixtures.
[0003] Since ZIF materials have rich metal and ligand varieties and are modifiable, they provide the potential for fine control of pore size and framework chemistry for the separation of different gases. It is a new strategy to precisely control the pore size of ZIF membranes for specific gas separations by mixing ligands. By introducing imidazole ligands of different sizes to exchange with the ligands in the initial ZIF material, mixed ligand ZIF materials are obtained, which can achieve the purpose of reducing and expanding the pore size of the ZIF membrane. Based on the developed ZIF membrane, the use of a mixed ligand strategy to achieve its separation of different gas mixtures is a simple and feasible method to obtain high-performance gas separation ZIF membranes. Summary of the invention
[0004] The present invention provides a method for preparing a mixed ligand MOF polycrystalline membrane. The preparation process of the mixed ligand MOF polycrystalline membrane provided by the present invention has simple operation and processing technology, good continuity, is dense and defect-free, and has excellent gas separation selectivity and stability.
[0005] The first object of the present invention is to provide a method for preparing a mixed ligand MOF polycrystalline film, the preparation method specifically comprising the following steps:
[0006] S1. Preparation of MOF membrane;
[0007] S2, performing a ligand exchange reaction on the MOF membrane prepared in step S1 and an organic imidazole to obtain a mixed ligand MOF polycrystalline membrane semi-finished product;
[0008] S3, activating the mixed ligand MOF polycrystalline membrane semi-finished product obtained in step S2 to obtain a mixed ligand MOF polycrystalline membrane.
[0009] Preferably, in step S1, the MOF membrane is selected from one of ZIF-7 membrane, ZIF-8 membrane, ZIF-62 membrane, ZIF-67, ZIF-90 membrane, ZIF-93 membrane, ZIF-97 membrane and ZIF-76 membrane.
[0010] Compared with the prior art, the present invention successfully reduces the pore size of the MOF membrane by introducing a ZIF-7 structure with a smaller pore size into the MOF membrane, thereby achieving efficient separation of small gases H2 / CH4, CO2 / CH4, and CO2 / N2; and introduces a ZIF-90 structure with a larger pore size into the MOF membrane, thereby enhancing the permeation flux of the MOF membrane to C3H6 / C3H8 and n-C4H8 / i-C4H8. The incorporation of the ZIF-8 structure into the ZIF-90 membrane achieves a significant improvement in the separation selectivity of n-C4H8 / i-C4H8 gases.
[0011] Furthermore, the preparation method of the ZIF-8 membrane specifically comprises the following steps:
[0012] ZIF-8 adopts the dip-coating thermal conversion method to prepare ZIF-8 membrane (patent CN 111841333 B). The ZIF-8 membrane prepared by this method has simple synthesis, high reproducibility, and excellent separation selectivity for macromolecular gases propylene and propane. By further reducing the concentration of the precursor solution, a high-throughput ZIF-8 membrane can be prepared (paper J.Membr.Sci.643(2022)
[0013] 120055). A high-throughput ZIF-8 membrane was prepared by controlling the concentration of the precursor solution, and organic ligand vapor treatment and conversion were performed under the high-throughput ZIF-8 membrane, thereby improving the gas permeability.
[0014] Further, the preparation method of the ZIF-90 membrane specifically includes the following steps: dissolving 0.577g of imidazole-2-carboxaldehyde in 15ml of methanol at 80°C, adding 0.66g of zinc acetate dihydrate after cooling to room temperature, stirring in an ice bath for 8min to obtain a ZIF-90 precursor solution, dipping the carrier in the precursor solution for 30s, taking it out and drying the water, reacting it in a 50°C blast oven for 30min, and naturally cooling to obtain a ZIF-90 amorphous layer, and steam-treating the ZIF-90 amorphous layer in a DMF solution at 80°C for 12h to obtain a ZIF-90 membrane. The ZIF-90 membrane is prepared by a steam conversion method (paper Chem. Eng. J. 496 (2024) 153737), and the ZIF-90 membrane prepared by this method has excellent separation performance for n-isobutane and propylene propane.
[0015] Preferably, the carrier used to prepare the MOF membrane can be selected from one of α-Al2O3 carrier, γ-Al2O3 carrier, anodized aluminum carrier, TiO2 carrier, PVDF carrier, PAN carrier, PES carrier, PTFE carrier and PEI carrier.
[0016] Preferably, in step S2, the specific steps of the ligand exchange reaction are as follows: placing an organic imidazole in a container, inverting the surface of the MOF membrane obtained in step S1 without direct contact with the organic imidazole, and performing a ligand exchange reaction.
[0017] Preferably, the temperature range of the ligand exchange reaction is 80° C. to 180° C., and the time of the ligand exchange reaction is 2 h to 48 h.
[0018] Compared with the prior art, the method of the present invention increases the volatilization of organic ligands by raising the temperature, controls the doping amount, and thus precisely regulates the effective separation pore size of the mixed ligand MOF polycrystalline membrane.
[0019] Preferably, the organic imidazole is one of benzimidazole, 2-aminobenzimidazole, 2-hydroxybenzimidazole, 2-hydroxymethylbenzimidazole, 5-methylbenzimidazole, imidazole, imidazole-2-carboxaldehyde, 4,5-dichloroimidazole, 2-nitroimidazole, 4-methylimidazole-5-carboxaldehyde, and 4-hydroxymethyl-5-methylimidazole.
[0020] Preferably, in step S3, the organic solvent is selected from one or more of dichloromethane, chloroform, acetone, methanol, ethanol, and dimethylformamide, and the activation treatment time is 3-6 hours.
[0021] The product after steam treatment needs to be solvent activated. In a preferred embodiment of the present invention, chloroform is used as an activator to activate the film after steam treatment. If there is no special explanation, the activation described in this specification is understood according to the conventional understanding, that is, the product to be activated is immersed in the activator for a period of time. As mentioned in this article, chloroform activation means immersing the product to be activated in chloroform for a specified time, which is 3 to 6 hours. Most of the full activation provided in our embodiments is 12 hours, but our related research also found that for the system of the present invention, activation for more than 3 hours, increasing the activation time does not significantly change the product performance. Therefore, the activation time can be selected according to the actual production within 3 to 6 hours. After solvent activation, it is further transferred to a 100°C vacuum oven for drying before testing.
[0022] Furthermore, the second aspect of the present invention provides a mixed ligand MOF polycrystalline film prepared by the above preparation method.
[0023] Furthermore, the third aspect of the present invention provides an application of the mixed ligand MOF polycrystalline membrane described in the second aspect, specifically separating the mixed ligand MOF polycrystalline membrane with a mixed gas.
[0024] Preferably, the mixed gas is selected from any one of carbon dioxide-methane mixed gas, carbon dioxide-nitrogen mixed gas, hydrogen-carbon dioxide mixed gas, hydrogen-methane mixed gas, helium-nitrogen mixed gas, helium-methane mixed gas, propylene-propane mixed gas, and n-butane-isobutane mixed gas. In summary, compared with the prior art, the present invention has the following advantages:
[0025] The steam ligand conversion provided by the present invention is used to prepare a dual-ligand MOF membrane, and the whole preparation process and processing technology are simple. The ligand used for steam treatment can be used repeatedly at a temperature of 140°C, and the mixed ligand MOF polycrystalline membrane has high repeatability, good economic applicability, and good gas separation ability. At the same time, the insertion of different MOFs enables the pore size of the original MOF to be precisely regulated, realizing the efficient separation of small gases and large gases. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is an X-ray diffraction characterization result diagram of the product C1 prepared in Example 1, the product M1 prepared in Example 1, the product M4 prepared in Example 1, and the product M7 prepared in Example 1 in a specific implementation manner of the present invention;
[0027] Figure 2 The surface result of scanning electron microscope characterization of product C4 (left picture) prepared in Example 1 and product M4 (right picture) prepared in Example 1 in a specific embodiment of the present invention;
[0028] Figure 3This is a single-component performance diagram of the product M4 gas obtained in Example 1 in a specific implementation manner of the present invention; DETAILED DESCRIPTION
[0029] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.
[0030] It should be noted that the endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.
[0031] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with conventionally understood meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents and instruments is carried out in accordance with the protocols and parameters given by the manufacturer.
[0032] It is worth mentioning that, in the present invention, the preparation method of the ZIF-8 membrane specifically comprises the following steps:
[0033] ZIF-8 adopts the dip-coating thermal conversion method to prepare ZIF-8 membrane (patent CN 111841333 B). The ZIF-8 membrane prepared by this method has simple synthesis, high reproducibility, and excellent separation selectivity for macromolecular gases propylene and propane. By further reducing the concentration of the precursor solution, a high-throughput ZIF-8 membrane can be prepared (paper J.Membr.Sci.643(2022)
[0034] 120055). A high-throughput ZIF-8 membrane was prepared by controlling the concentration of the precursor solution, and organic ligand vapor treatment and conversion were performed under the high-throughput ZIF-8 membrane, thereby improving the gas permeability.
[0035] Further, the preparation method of the ZIF-90 membrane specifically includes the following steps: dissolving 0.577g of imidazole-2-carboxaldehyde in 15ml of methanol at 80°C, adding 0.66g of zinc acetate dihydrate after cooling to room temperature, stirring in an ice bath for 8min to obtain a ZIF-90 precursor solution, dipping the carrier in the precursor solution for 30s, taking it out and drying the water, reacting it in a 50°C blast oven for 30min, and naturally cooling to obtain a ZIF-90 amorphous layer, and steam-treating the ZIF-90 amorphous layer in a DMF solution at 80°C for 12h to obtain a ZIF-90 membrane. The ZIF-90 membrane is prepared by a steam conversion method (paper Chem. Eng. J. 496 (2024) 153737), and the ZIF-90 membrane prepared by this method has excellent separation performance for n-isobutane and propylene propane.
[0036] The technical effects of the present invention are described below in conjunction with specific embodiments.
[0037] Example 1
[0038] This embodiment provides a method for preparing a ZIF-8-7 membrane, which is as follows:
[0039] 1.32 g (15 mmol) Zn(OAc)2·2H2O and 1 g 2-methylimidazole were added to 15 ml H2O / DMAC (2 / 1) solution, marked as solution A and solution B, respectively. After stirring in an ice bath for 8 minutes, solution B was added to solution A within 90 s. After stirring for 30 s, a precursor solution of ZIF-8 membrane was obtained. The Al2O3 carrier was dipped in the precursor solution for 30 s, taken out and dried, and reacted in a 200°C forced air oven for 15 min. After natural cooling, ZIF-8 polycrystalline membranes were obtained, which were marked as C1 to C9, respectively.
[0040] Take 0.2g of benzimidazole and place it in a small bottle. Invert the surface of the C1-C9 membrane (not in direct contact with the ligand). React C1-C3 in a 80℃ forced air oven for 12h, react C4-C6 in a 100℃ forced air oven for 12h, and react C7-C9 in a 120℃ forced air oven for 12h.
[0041] C1-C9 were taken out, activated in 10 ml of chloroform for 2 h, and then vacuum activated in a vacuum oven at 100° C. for 12 h. These products were recorded as products M1-M9.
[0042] The results of the carbon dioxide / methane separation selectivity and permeability test of products C1~C9 and M1~M9 are shown in Table 1-1 and Table 1-2. Comparing the performance data before and after modification, the doping of ZIF-7 effectively reduced the effective separation pore size of the ZIF-8 membrane, and the ZIF-8-7 membrane has excellent carbon dioxide and methane separation performance.
[0043] The results of hydrogen / methane separation selectivity and permeability test for products C7~C9 and M7~M9 are shown in Tables 1-3 and 1-4. The results of helium / nitrogen separation selectivity and permeability test are shown in Tables 1-5 and 1-6. Comparing the performance data before and after modification, the high-doped ZIF-8-7 membrane has excellent hydrogen / methane and helium / nitrogen separation performance at a higher benzimidazole volatilization temperature.
[0044] Table 1-1: Carbon dioxide / methane separation selectivity and permeability test results of products C1 to C9
[0045]
[0046] Table 1-2: Carbon dioxide / methane separation selectivity and permeability test results of products M1 to M9
[0047]
[0048]
[0049] Table 2-3: Hydrogen / methane separation selectivity and permeability test results of products C7 to C9
[0050]
[0051] Table 1-4: Hydrogen / methane separation selectivity and permeability test results of products M7~M9
[0052]
[0053] Table 3-5: Helium / nitrogen separation selectivity and permeability test results of products C7 to C9
[0054]
[0055] Table 1-6: Helium / nitrogen separation selectivity and permeability test results of products M7~M9
[0056]
[0057]
[0058] Example 2
[0059] This embodiment provides a method for preparing a high-throughput ZIF-8-7 membrane, which specifically comprises the following steps:
[0060] 0.33 g Zn(OAc)2·2H2O and 0.25 g 2-methylimidazole were added to 15 ml H2O / DMAC (2 / 1) solution, marked as solution A and solution B, respectively. After stirring in an ice bath for 8 minutes, solution B was added to solution A within 90 seconds. After stirring for 30 seconds, a precursor solution of high-flux ZIF-8 membrane was obtained. The Al2O3 carrier was dipped in the precursor solution for 30 seconds, taken out and dried, and reacted in a 200°C forced air oven for 15 minutes. After natural cooling, a high-flux ZIF-8 polycrystalline membrane was obtained, marked as C and B. 10 , C 11 , C 12 .
[0061] Take 0.2g of benzimidazole and place it in a small bottle. 10 , C 11 , C 12 The membrane surface was inverted (not in direct contact with the ligand) and reacted in a forced air oven at 100°C for 12 h.
[0062] C 10 ~C 12 Take it out, activate it in 10 ml of chloroform for 2 h, and activate it in a vacuum oven at 100 ° C for 12 h, which are respectively recorded as product M 10 , Product M 11 and product M 12 .
[0063] Product C 10 ~C 12 and M 10 ~M 12 The results of the carbon dioxide / methane separation selectivity and permeability test are shown in Tables 2-1 and 2-2. The carbon dioxide / methane selectivity has been improved, and the carbon dioxide permeability has also been significantly improved.
[0064] Table 2-1: Product C 10 ~C 12 Table of test results of carbon dioxide / methane separation selectivity and permeability
[0065]
[0066] Table 2-2: Product M 10 ~M 12 Table of test results of carbon dioxide / methane separation selectivity and permeability
[0067]
[0068]
[0069] Example 3
[0070] This embodiment provides a method for preparing a ZIF-8-90 membrane, which specifically comprises the following steps:
[0071] 1.32 g Zn(OAc)2·2H2O and 1 g 2-methylimidazole were added to 15 ml H2O / DMAC (2 / 1) solution, marked as solution A and solution B, respectively. After stirring in an ice bath for 8 minutes, solution B was added to solution A within 90 seconds. After stirring for 30 seconds, a precursor solution of high-flux ZIF-8 membrane was obtained. The Al2O3 carrier was dipped in the precursor solution for 30 seconds, taken out and dried, and reacted in a 200°C forced air oven for 15 minutes. After natural cooling, a high-flux ZIF-8 polycrystalline membrane was obtained, marked as C and B. 13 , C 14 , C 15 .
[0072] Take 0.2g of imidazole-2-carboxaldehyde and place it in a small bottle. 13 , C 14 , C 15 The membrane surface was inverted (not in direct contact with the ligand) and reacted in a forced air oven at 100°C for 12 h.
[0073] C 13 ~C 15 Take it out, activate it in 10 ml of chloroform for 2 h, and activate it in a vacuum oven at 100 ° C for 12 h, which are respectively recorded as product M 13 , Product M 14 and product M 15 .
[0074] Product C 13 ~C 15 and M 13 ~M 15 The propylene / propane separation selectivity and permeability test results are shown in Tables 3-1 and 3-2. After doping with ZIF-90, the propylene propane flux of the ZIF-8-90 membrane was improved.
[0075] Table 3-1: C 13 ~C 15 Propylene / propane separation selectivity and permeability test results table
[0076]
[0077] Table 3-2: M 13 ~M 15 Propylene / propane separation selectivity and permeability test results table
[0078]
[0079]
[0080] Example 4
[0081] This embodiment provides a method for preparing a ZIF-90-8 membrane, which specifically comprises the following steps:
[0082] 0.577g of imidazole-2-carboxaldehyde was dissolved in 15ml of methanol at 80℃, cooled to room temperature, added with 0.66g of zinc acetate dihydrate, stirred in an ice bath for 8min to obtain a ZIF-90 precursor solution, the carrier was dipped in the precursor solution for 30s, taken out and dried, and reacted in a 50℃ forced air oven for 30min, and naturally cooled to obtain a ZIF-90 amorphous layer, and the ZIF-90 amorphous layer was treated with DMF solution at 80℃ steam for 12h to obtain a ZIF-90 membrane. They are denoted as C 16 , C 17 , C 18 .
[0083] Take 0.2g of 2-methylimidazole and place it in a small bottle. 16 , C 17 , C 18 The membrane surface was inverted (not in direct contact with the ligand) and reacted in a forced air oven at 100°C for 12 h.
[0084] C 16 ~C 18 Take out, activate in 10ml methanol for 2h, and record as product M 16 , Product M 17 and product M 18 .
[0085] Product C 16 ~C 18 and M 16 ~M 18 The results of n-isobutane separation selectivity and permeability test are shown in Tables 4-1 and 4-2. After doping with ZIF-8, the selectivity of ZIF-90-8 membrane for n-isobutane is improved.
[0086] Table 4-1: C 16 ~C 18 Table of n-butane / isobutane separation selectivity and permeability test results
[0087]
[0088] Table 4-2: M 16 ~M 18 Table of n-butane / isobutane separation selectivity and permeability test results
[0089]
[0090] By comparing the separation performance before and after the exchange, it can be seen that the mixed ligand MOF polycrystalline membrane achieves precise control of the pore size. Doping ZIF-7 in the ZIF-8 membrane effectively reduces the pore size of the membrane, which is suitable for the separation of small-sized gases such as hydrogen and carbon dioxide. Doping ZIF-90 effectively expands the pore size of the membrane, which is suitable for the separation of large-sized propylene gases, and increases the permeation flux of propylene by nearly 5 times. Doping ZIF-8 in the ZIF-90 membrane effectively reduces the pore size of the membrane, and improves the separation selectivity of n-butane gas.
[0091] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with commonly understood meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be understood to represent significant differences from the conventional understanding of the art.
[0092] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a mixed ligand MOF polycrystalline film, characterized in that: The preparation method specifically comprises the following steps: S1. Preparation of MOF membrane; S2, subjecting the MOF membrane prepared in step S1 to a ligand exchange reaction with an organic imidazole ligand to obtain a mixed ligand MOF polycrystalline membrane semi-finished product; S3, activating the mixed ligand MOF polycrystalline membrane semi-finished product obtained in step S2 to obtain a mixed ligand MOF polycrystalline membrane.
2. The method for preparing a mixed ligand MOF polycrystalline film according to claim 1, characterized in that: In the step S1, the MOF membrane is selected from one of a ZIF-7 membrane, a ZIF-8 membrane, a ZIF-62 membrane, a ZIF-67 membrane, a ZIF-90 membrane, a ZIF-93 membrane, a ZIF-97 membrane, and a ZIF-76 membrane.
3. The method for preparing a mixed ligand MOF polycrystalline film according to claim 1, characterized in that: In step S2, the specific steps of the ligand exchange reaction are as follows: placing an organic imidazole ligand in a container, inverting the surface of the MOF membrane obtained in step S1 without direct contact with the organic imidazole, and performing a ligand exchange reaction.
4. The method for preparing a mixed ligand MOF polycrystalline film according to claim 3, characterized in that: The temperature range of the ligand exchange reaction is 60° C. to 180° C., and the time range of the ligand exchange reaction is 2 h to 48 h.
5. The method for preparing a mixed ligand MOF polycrystalline film according to claim 1, characterized in that: The organic imidazole ligand is selected from one of benzimidazole, 2-aminobenzimidazole, 2-hydroxybenzimidazole, 2-hydroxymethylbenzimidazole, 5-methylbenzimidazole, imidazole, imidazole-2-carboxaldehyde, 4,5-dichloroimidazole, 2-nitroimidazole, 4-methylimidazole-5-carboxaldehyde, and 4-hydroxymethyl-5-methylimidazole.
6. The method for preparing a mixed ligand MOF polycrystalline film according to claim 1, characterized in that: In step S3, the organic solvent for activation treatment is selected from one or more of dichloromethane, chloroform, acetone, methanol, ethanol, and dimethylformamide, the activation treatment time is 3-24 hours, and the activation treatment temperature is 25-80°C.
7. A mixed ligand MOF polycrystalline film, characterized in that: The method is prepared by any one of claims 1 to 6.
8. An application of the mixed ligand MOF polycrystalline film according to claim 7, characterized in that: The mixed-ligand MOF polycrystalline membrane was used for mixed gas separation.
9. The use according to claim 8, characterized in that The mixed gas is selected from any one of carbon dioxide-methane mixed gas, carbon dioxide-nitrogen mixed gas, hydrogen-carbon dioxide mixed gas, hydrogen-methane mixed gas, helium-nitrogen mixed gas, helium-methane mixed gas, propylene-propane mixed gas, and n-butane-isobutane mixed gas.