Mesoporous high polymer material based on organic-inorganic interaction of porous silicon dioxide interface as well as preparation method and application of mesoporous high polymer material

Through the surface infusion method of porous silica interface organic-inorganic interaction, the strict requirements and structural collapse problems in the synthesis of mesoporous polymer materials are solved, and mesoporous polymer materials with high specific surface area and large pore volume are prepared. In the fields of catalysis and biomedical science, the stability and wide application of materials have been improved.

CN119081214APending Publication Date: 2024-12-06WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085452.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing synthesis methods of mesoporous polymer materials have harsh polymer block copolymer requirements, difficult to control the sol-gel process, structural collapse and guide agent residues, resulting in low specific surface area and porosity, which limits its application. .

Method used

Using the surface perfusion method based on the interfacial organic-inorganic interaction of porous silica, the mesoporous polymer with hollow structure is selectively polymerized on the nanopore surface through the interaction of the mesoporous silica template and the organic molecular precursor. Material preparation, the second polymerization temperature is controlled to retain the polymer structure and increase the pore volume.

Benefits of technology

Mesoporous polymer materials with high specific surface area and large pore volume are prepared, which are suitable for catalysis, adsorption and biomedical fields, improving the stability of catalysts and the wide range of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081214A_ABST
    Figure CN119081214A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a mesoporous high polymer material based on organic-inorganic interaction of a porous silicon dioxide interface, which innovatively adopts a surface perfusion method, takes mesoporous silicon dioxide as a template, fills different organic molecule precursors into the silicon dioxide template, and firstly prepares a polymer / mesoporous silicon dioxide compound; and carrying out thermal polymerization reaction, and finally etching off the silicon dioxide template to obtain the hollow-structure mesoporous high polymer material with high specific surface area and large pore volume. The prepared hollow-structure mesoporous polymer material has high surface area and large pore volume, retains the characteristics of a polymer structure, can be modified and functionalized, has more abundant and diversified structures, is suitable for the fields of catalysis, adsorption, biological medicine and the like, and can be used as a carrier in a heterogeneous catalyst to improve the catalytic activity of the catalyst. The catalyst prepared by the method can promote interaction with metal active components, plays a role in serving as a ligand, effectively improves the stability of the catalyst, and has popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomaterials, and specifically relates to a mesoporous polymer material based on organic-inorganic interaction at the porous silica interface and a preparation method thereof, and also relates to the application of the mesoporous polymer material as a catalyst carrier. Background Art

[0002] Mesoporous polymer materials have excellent properties such as high stability, easy modification, high specific surface area and large pore volume. They are widely used in many fields such as catalyst supports, gas adsorbents, gas storage materials and electrode materials, and even have important applications in the biomedical field.

[0003] At present, the synthesis methods of mesoporous polymers are mainly divided into amphiphilic molecular self-assembly method, soft template method and hard template method. However, the amphiphilic molecular self-assembly method for synthesizing mesoporous polymer materials is extremely demanding on the selected polymer block copolymers, and there are only a few successful cases; the preparation by the soft template method has the problems of difficult control of the sol-gel process, the removal of the soft template easily leads to structural collapse and the residue of the structure-directing agent, which limits its wide application; the traditional hard template method for synthesizing mesoporous polymers can avoid the problems of the above two methods to a certain extent, but filling and polymerizing organic molecules in the nanopores of the hard template often requires filling the pores to support the organic skeleton structure after the template is removed. Therefore, the obtained mesoporous polymer materials often have low specific surface area and porosity, and the organic molecular precursors that can successfully obtain the porous skeleton structure are very limited, which greatly limits the application and development of mesoporous polymer materials.

[0004] Based on this, it is an urgent technical problem to provide a universal new method to prepare mesoporous polymer materials with high stability, high specific surface area and larger pore volume to meet the application needs in fields such as catalysis, adsorption or biomedicine. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for preparing a mesoporous polymer material based on organic-inorganic interaction at the porous silica interface.

[0006] The second object of the present invention is to provide a mesoporous polymer material based on organic-inorganic interaction at the porous silica interface.

[0007] The third object of the present invention is to provide an application of a mesoporous polymer material based on organic-inorganic interaction at the porous silica interface.

[0008] The technical solution adopted by the present invention to achieve one of the purposes is: to provide a method for preparing a mesoporous polymer material based on organic-inorganic interaction at the interface of porous silica, comprising the following steps: S1, mixing a polymer precursor with a solvent to obtain a precursor solution; the polymer precursor includes a combination of one or more of resol phenolic resin, furfuryl alcohol, 2-thiophene methanol, pyrrole, dopamine, thiophene, cyanamide, aniline, styrene, and pyridine; S2, dropping the precursor solution into the mesoporous silica template, and performing a first polymerization reaction at 25-150° C. to obtain a polymer / mesoporous silica composite; S3, placing the polymer / mesoporous silica composite under an inert atmosphere and performing a second polymerization reaction at 200-480° C.; then etching the silica template, washing and drying the product to obtain a mesoporous polymer material with a hollow structure.

[0009] The general idea of ​​the present invention is as follows: In order to solve the problems existing in the existing mesoporous polymer synthesis methods, the present invention innovatively uses a "surface perfusion method" to synthesize a mesoporous polymer material with a hollow structure. The method utilizes the interaction between the abundant silanol groups on the surface of mesoporous silica and the organic molecular precursors to selectively polymerize the organic molecules on the surface of the nanopores, and by changing the amount of the organic molecular precursors filled into the mesoporous silica, a layer of polymer material is selectively coated in the nanopore confined space. Then, the silica template is removed to obtain a mesoporous polymer material with a hollow structure, and the inner and outer surfaces of the cavity can contribute to the surface area and have two sets of pore size distributions at the same time. Therefore, the mesoporous polymer material obtained by the present invention has a higher specific surface area and a larger pore volume. In addition, the preparation method provided by the present invention has a wide range of applicability, and the method can be extended to a variety of organic molecular precursors, such as resol phenolic resin, furfuryl alcohol, 2-thiophene methanol, pyrrole, dopamine, thiophene, cyanamide, aniline, styrene and pyridine, etc., to prepare hollow structure mesoporous polymer materials with different polymer skeletons.

[0010] In the above preparation method, a staged polymerization method is adopted. First, the first polymerization reaction is carried out at 25-150°C to polymerize the organic precursor molecules into a polymer structure; then, the second polymerization reaction is carried out at 200-480°C in an inert atmosphere or under vacuum conditions to volatilize some impurities and small organic molecules, thereby completing the preparation of the hollow structure mesoporous polymer material.

[0011] In the present invention, the second polymerization reaction temperature is controlled to be 200-480°C, which can not only prepare a mesoporous material with a relatively high specific surface area and a large pore volume, but also retain the characteristics of the polymer structure (avoiding carbonization caused by excessively high temperature). The polymer structure present in the mesoporous material can not only be modified and functionalized to make its structure more diverse; but also as a carrier in a heterogeneous catalyst, it can promote the interaction with the metal active component, solve the problem of metal nanoparticle aggregation in the catalytic reaction process, and thus effectively improve the stability of the catalyst.

[0012] Furthermore, in step S1, the precursor solution also includes a catalyst; the catalyst includes one or more combinations of ferric chloride, oxalic acid, ferric nitrate, cupric chloride, cupric nitrate, ferric nitrate, ammonium persulfate, tin chloride, and aluminum chloride.

[0013] Furthermore, in step S1, the solvent includes a combination of one or more of anhydrous ethanol, methanol, water, trimethylbenzene, ethylbenzene, n-hexane, N,N-dimethylformamide, dichloroethane, and 1,2-dichlorobenzene.

[0014] Preferably, in the precursor solution, the mass concentration of the polymer precursor is 30 wt.%-60 wt.%.

[0015] Further, in step S2, the mesoporous silica template includes a combination of one or more of SBA-15-OH, MCF-OH, KIT-6-OH, SBA-12-OH, FDU-12-OH and SBA-16-OH.

[0016] Furthermore, in step S2, the mass volume ratio of the mesoporous silica template to the precursor solution is 1: (1-5) g / mL.

[0017] Furthermore, in step S2, the second polymerization reaction is carried out under nitrogen, argon or vacuum conditions.

[0018] Furthermore, when the polymer precursor is selected from one of resol phenolic resin, aniline, styrene, and dopamine, before step S3, the following operation is also included: mixing the polymer / mesoporous silica composite obtained in step S2 with a crosslinking agent and a catalyst, and performing a crosslinking reaction at 70-130° C. for 12-48 h to obtain a crosslinked polymer / mesoporous silica composite.

[0019] In the present invention, by cross-linking the polymer / mesoporous silica composite, the specific surface area of ​​the hollow mesoporous polymer material can be further increased, and the skeleton structure of the polymer material can be strengthened to avoid the reduction of porosity caused by pore collapse or swelling of the mesoporous polymer material in the solvent during application.

[0020] Preferably, the cross-linking agent includes a combination of one or more of benzyl dichloride, ethylene dichloride, 1-bromopropane, and 1-chloropropane; the catalyst includes a combination of one or more of ferric chloride, oxalic acid, ferric nitrate, cupric chloride, cupric nitrate, ferric nitrate, ammonium persulfate, tin chloride, and aluminum chloride.

[0021] Preferably, the mass ratio of the polymer / mesoporous silica composite, the catalyst and the cross-linking agent is 25:(4-6):(0.5-1.5).

[0022] Furthermore, in step S3, the solvent used in the etching process includes a combination of one or more of hydrofluoric acid, sodium hydroxide solution or potassium hydroxide solution. Preferably, the volume concentration of hydrofluoric acid is 0.1-40 vol.%, the concentration of sodium hydroxide solution is 0.1-10 mol / L, and the concentration of potassium hydroxide solution is 0.1-10 mol / L.

[0023] Furthermore, in step S3, the drying process is performed by freeze drying, the freeze drying temperature is -90 to -40°C, and the freeze drying time is 1-48 hours.

[0024] The technical solution adopted by the present invention to achieve the second purpose is: to provide a mesoporous polymer material based on organic-inorganic interaction at the interface of porous silica, which is prepared by the preparation method described in one of the purposes of the present invention.

[0025] Furthermore, the specific surface area of ​​the mesoporous polymer material prepared by the present invention is 271-888m 2 / g, pore volume 0.3-1.4cm 3 / g; the mesoporous polymer material has two sets of pore size distributions, and the average pore size distribution is in the range of 2.4-4.7nm and 17-27nm.

[0026] The mesoporous polymer material prepared by the present invention realizes a hollow structure at the nanoscale, so that the surface groups are fully exposed and have a larger specific surface area and pore volume. The mesoporous polymer material retains the characteristics of the polymer structure, is easier to modify and functionalize, and makes its structure more diverse. Its structure and properties can be adjusted to meet the application requirements of different fields.

[0027] The technical solution adopted by the present invention to achieve the third purpose is to provide an application of the mesoporous polymer material based on the organic-inorganic interaction at the porous silica interface according to the second purpose of the present invention. The mesoporous polymer material prepared by the present invention can be widely used in the fields of catalysis, adsorption and biomedicine.

[0028] Furthermore, the mesoporous polymer material is applied in the field of catalysis. As a carrier in a heterogeneous catalyst, it can enhance the interaction with the metal active components, solve the problems of metal nanoparticle leaching and aggregation in the catalytic reaction process, and effectively improve the stability of the catalyst; it can be sulfonated and aminated, and directly used as an acid-base catalyst to catalyze organic reactions.

[0029] Furthermore, the mesoporous polymer material is applied in the biomedical field. It has good compatibility with biological tissues and can be used as a carrier of artificial organs and tissue repair materials, such as a scaffold for sutures or artificial tissues.

[0030] Furthermore, the mesoporous polymer material is applied in the field of adsorption, and the hydroxyl groups on the mesoporous polymer are used to form hydrogen bonds with methylene blue molecules to enhance the adsorption of dye molecules; and the hydroxyl groups and amino groups on the mesoporous polymer are used to adsorb heavy metal chromium ions.

[0031] Preferably, the application includes: using the mesoporous polymer material as a carrier to load precious metals to prepare a catalyst, and applying the catalyst to the transfer catalytic hydrogenation reaction of benzaldehyde compounds.

[0032] Furthermore, the transfer catalytic hydrogenation reaction of the benzaldehyde compound is carried out under normal pressure, a reaction temperature of 80-130° C., and a hydrogen source of isopropanol. Preferably, in the catalyst, the precursor of the mesoporous polymer material is 2-thiophene methanol, and the noble metal is palladium.

[0033] Compared with the prior art, the present invention has the following beneficial effects: (1) The preparation method of mesoporous polymer materials based on organic-inorganic interaction at the porous silica interface provided by the present invention adopts the "surface perfusion method" to synthesize mesoporous polymer materials with hollow structures. By enhancing the interaction between the surface groups of the nanopores of the silica template and the organic molecules, the organic molecules are selectively polymerized on the surface of the nanopores, and a layer of polymer material is selectively coated in the confined space of the nanopores; then, the silica template is removed to obtain a mesoporous polymer material with a hollow structure, the inner and outer surfaces of which can contribute to the surface area and have two sets of pore size distributions at the same time. This method has general applicability to a variety of organic molecular precursors, such as resol phenolic resin, furfuryl alcohol, 2-thiophene methanol, pyrrole, dopamine, thiophene, monocyanamide, aniline, styrene and pyridine.

[0034] (2) The mesoporous polymer material based on the organic-inorganic interaction at the porous silica interface prepared by the present invention has high stability, high specific surface area and larger pore volume. The mesoporous polymer material retains the characteristics of the polymer structure and can be modified and functionalized to make its structure more diverse.

[0035] (3) The mesoporous polymer material based on the organic-inorganic interaction at the porous silica interface prepared by the present invention has broad promotion and application prospects in the fields of catalysis, adsorption and biomedicine. The mesoporous polymer material, as a carrier in a heterogeneous catalyst, can promote the interaction with the metal active component, act as a ligand, and effectively improve the stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The nitrogen adsorption-desorption isotherm of the hollow structure mesoporous phenolic resin prepared in Example 1 of the present invention; Figure 2 is the pore size distribution curve of the hollow structure mesoporous phenolic resin prepared in Example 1 of the present invention; Figure 3 The hollow structure mesoporous phenolic resin prepared in Example 1 of the present invention 13 C NMR spectroscopy; Figure 4 This is a nitrogen adsorption-desorption curve of the highly cross-linked hollow structure mesoporous phenolic resin prepared in Example 2 of the present invention; Figure 5 This is a transmission electron microscope photograph of the highly cross-linked hollow structure mesoporous phenolic resin prepared in Example 2 of the present invention; Figure 6 This is a scanning electron micrograph of the hollow structure mesoporous polyfurfuryl alcohol prepared in Example 3 of the present invention; Figure 7 This is a transmission electron microscope photograph of the hollow structure mesoporous polyfurfuryl alcohol prepared in Example 3 of the present invention; Figure 8 This is an optical photograph of the hollow structure mesoporous polyfurfuryl alcohol prepared in Example 3 of the present invention; Fig. 9 This is a scanning electron micrograph of the hollow structure mesoporous polypyrrole prepared in Example 4 of the present invention; Fig.10 This is a transmission electron microscope photograph of the hollow structure mesoporous polypyrrole prepared in Example 4 of the present invention; Fig.11 is the Fourier transform infrared spectrum curve of the hollow structure mesoporous polypyrrole prepared in Example 4 of the present invention; Fig.12 This is the nitrogen adsorption-desorption isotherm of the hollow structure mesoporous polythiophene methanol prepared in Example 5 of the present invention; Fig.13 This is the pore size distribution curve of the hollow structure mesoporous polythiophene methanol prepared in Example 5 of the present invention; Fig.14 This is an optical photograph of the hollow structure mesoporous polythiophene methanol prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0039] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0040] The preparation method of mesoporous silica MCF-OH used in each embodiment of the present invention comprises the following steps: Step 1: Use a balance to weigh 20.0 g of the polyether block copolymer P123 into a 1000 mL wide-mouth bottle, then add 1.6 mol / L hydrochloric acid and place in a 38 °C water bath for dissolution.

[0041] Step 2: Then add 20.0 g of mesitylene and 0.23 g of ammonium fluoride, stir continuously for 1 h, then add 41.6 g of tetraethyl orthosilicate, and continue stirring for 24 h.

[0042] Step 3: After the reaction is completed, three quarters of the milky white liquid in the bottle is filtered, and then transferred to a hydrothermal kettle together with the remaining mother liquor, and hydrothermaled at 110 ° C for 24 h. After the reaction is completed, cool to room temperature, filter the reactant and dry it to obtain a white solid powder.

[0043] Step 4: Weigh 8.0 g of the above white powder into a 1000 mL round-bottom flask, then add hydrogen peroxide (35 wt.%) and concentrated nitric acid (65 wt.%) in sequence. Place it at 80 °C for 3 h, and absorb the tail gas with NaOH. After cooling to room temperature, filter the liquid after the reaction, wash and dry to obtain foamy mesoporous silica MCF-OH with rich silanol groups on the surface.

[0044] Example 1 This embodiment provides a hollow structure mesoporous phenolic resin, and the preparation method thereof comprises the following steps: Step 1: Dilute 70 wt.% resol solution to 40 wt.% with anhydrous 1,2-dichlorobenzene.

[0045] The preparation process of the resol phenolic resin solution is as follows: 32.0 g of phenol is heated and melted in a 250 mL round-bottom flask, 20 wt.% NaOH solution is added, and after reacting for 10 minutes, 56.64 g of formalin aqueous solution (37 wt.%) is added, and then the temperature is raised to 70 °C and kept at this temperature for 1 hour. After cooling to room temperature, the pH value is adjusted to 7.0 with hydrochloric acid, and then the water in the solution is removed. And anhydrous ethanol is used to prepare a 70 wt.% resol phenolic resin solution.

[0046] Step 2: Weigh 0.5 g of the pre-vacuum-dried MCF-OH template into a 20 mL glass bottle, add a total of 1.1 mL of the resol solution three times, and stir thoroughly. Then place the 20 mL glass bottle in a 1000 mL wide-mouth bottle for the first polymerization reaction, heat to 130 °C and keep warm for 48 h. Subsequently, evaporate the solvent in a fume hood to obtain a phenolic resin / MCF-OH composite.

[0047] Step 3: The composite obtained in step 2 was subjected to vacuum polymerization in a tube furnace, heated to 350 °C at a heating rate of 5 °C / min, and maintained at this temperature for 48 h. After cooling to room temperature, the silica template was removed using a 10 wt.% hydrofluoric acid solution. Finally, the product was freeze-dried to obtain a yellow powder.

[0048] The specific surface area of ​​the hollow structure mesoporous phenolic resin prepared in this example is 646 m 2 / g, pore volume 1.4 cm 3 / g, with a bi-pore distribution of average pore sizes of 3.4 nm and 26.4 nm. Its nitrogen adsorption-desorption isotherm, pore size distribution curve and 13 C NMR spectroscopy Figure 1 , Figure 2 and Figure 3 shown.

[0049] Example 2 The difference between this embodiment and embodiment 1 is that the phenolic resin / MCF-OH composite obtained in step 2 is cross-linked (the phenolic resin / MCF-OH composite obtained in step 1 of embodiment 1 is mixed with benzyl chloride and anhydrous ferric chloride in a mass ratio of 25:5:1, stirred thoroughly, placed in a forced air drying oven, reacted at 70-130 ° C. for 12-48 h, and cooled to room temperature). Then in step 3, the cross-linked composite is vacuum thermally polymerized by the same method as in embodiment 1, and the silica template is etched to remove, thereby obtaining a highly cross-linked hollow structure mesoporous phenolic resin.

[0050] The specific surface area, pore volume and pore size of the hollow structure mesoporous phenolic resin prepared under different cross-linking temperatures and cross-linking times were tested, and the results are shown in Table 1 below.

[0051] Table 1

[0052] It can be seen from Table 1 above that The use of a crosslinking agent can increase the structure of the polymer skeleton and make it more stable. Furthermore, the temperature and time of crosslinking will also affect the specific surface area and pore size distribution of the mesoporous polymer material. For the highly crosslinked hollow structure mesoporous phenolic resin prepared by the present invention, when the crosslinking temperature is controlled to be 130°C and the crosslinking time is 24h, the highly crosslinked hollow structure mesoporous phenolic resin has the best comprehensive performance, and its specific surface area is 888 m 2 / g, pore volume 1.2cm 3 / g, with a bi-pore distribution of average pore diameters of 4.7 nm and 25.3 nm. The nitrogen adsorption-desorption isotherms and transmission electron micrographs of the highly cross-linked hollow structure mesoporous phenolic resin prepared in this example are shown in FIG. Figure 4 and Figure 5 shown.

[0053] Example 3 This embodiment provides a hollow structure mesoporous polyfurfuryl alcohol, and the preparation method thereof comprises the following steps: Step 1: Mix 4 mL of furfuryl alcohol and 4 mL of mesitylene, then add 20 mg of oxalic acid dihydrate and stir to dissolve.

[0054] Step 2: Weigh 0.5 g of the pre-vacuum-dried MCF-OH template into a 20 mL glass bottle, add 1.542 mL of the above furfuryl alcohol solution, and stir thoroughly. Then place the 20 mL glass bottle in a 1000 mL wide-mouth bottle for polymerization, first heating at 50 °C for 24 h, and then polymerizing at 90 °C for 48 h. Afterwards, evaporate the solvent in a fume hood to obtain the furfuryl alcohol / MCF-OH complex.

[0055] Step 3: The obtained composite was vacuum polymerized in a tube furnace, heated to 350 °C at a heating rate of 5 °C / min, and maintained at this temperature for 48 h. After cooling to room temperature, the silica template was removed using a 10 wt.% hydrofluoric acid solution or a 2 mol / L sodium hydroxide solution. Finally, the product was freeze-dried to obtain a reddish-brown powder.

[0056] The specific surface area of ​​the hollow structure mesoporous polyfurfuryl alcohol prepared in this example is 545 m 2 / g, pore volume 1.0 cm 3 / g, with a double pore distribution of average pore diameters of 2.4 nm and 21.8 nm. Its scanning electron micrographs, transmission electron micrographs and optical photographs are shown in Figure 6 , Figure 7 and Figure 8 shown.

[0057] Example 4 This embodiment provides a hollow structure mesoporous polypyrrole, and the preparation method thereof comprises the following steps: Step 1: Use a pipette to transfer 1 mL of pyrrole and 1 mL of 1,2-dichlorobenzene into a 20 mL glass bottle.

[0058] Step 2: Weigh 0.5 g of the pre-vacuum-dried MCF-OH template into a 20 mL glass bottle, add 1.542 mL of the above pyrrole solution, and stir thoroughly. Then weigh 20 mg of FeCl3 and add it to the stirred powder, and stir thoroughly again. Then place the glass bottle in a 1000 mL wide-mouth bottle for polymerization at 130 ° C for 48 h. After it cools naturally, open the bottle cap in the glass bottle and place it in a fume hood to evaporate the solvent to obtain a pyrrole / MCF-OH complex.

[0059] Step 3: The obtained composite was vacuum polymerized in a tube furnace, heated to 450 °C at a heating rate of 2 °C / min, and maintained at this temperature for 300 min. After cooling to room temperature, the silica template was removed using a 10 wt.% hydrofluoric acid solution. Finally, the obtained product was freeze-dried to obtain a black powder.

[0060] The specific surface area of ​​the hollow mesoporous polypyrrole prepared in this example is 271 m 2 / g, pore volume 0.3 cm 3 / g, with an average pore size of 2.8 nm and a double pore distribution of 17.8 nm. Its scanning electron micrograph, transmission electron micrograph and Fourier transform infrared spectrum curve are shown in Fig. 9 , Fig.10 and Fig.11 shown.

[0061] Example 5 This embodiment provides a hollow structure mesoporous polythiophene methanol, and the preparation method thereof comprises the following steps: Step 1: Dissolve 40 mg Fe(NO3)3.9H2O in a mixed solution consisting of 2 mL thiophene methanol, 1.6 mL 1,2-dichlorobenzene and 0.4 mL ethanol and stir at room temperature for 30 min.

[0062] Step 2: Weigh 0.5 g of the pre-vacuum-dried MCF-OH template into a 20 mL glass bottle, add 1.542 mL of the above thiophene methanol solution, and stir thoroughly. Then place the glass bottle in a 1000 mL wide-mouth bottle for polymerization at 130 °C for 48 h. After cooling naturally, open the glass bottle cap and place it in a fume hood to evaporate the solvent to obtain thiophene methanol / MCF-OH composite.

[0063] Step 3: The obtained composite was vacuum polymerized in a tube furnace, heated to 350 °C at a heating rate of 5 °C / min, and maintained at this temperature for 48 h. After cooling to room temperature, the silica template was removed using a 10 wt.% hydrofluoric acid solution. Finally, the obtained product was freeze-dried to obtain a brown powder.

[0064] The specific surface area of ​​the hollow mesoporous polythiophene methanol prepared in this example is 521 m 2 / g, pore volume 1.1cm 3 / g, with a bi-pore distribution of average pore sizes of 3.4 nm and 27.8 nm. Its nitrogen adsorption-desorption isotherm, pore size distribution curve and optical photographs are shown in Figure 2. Fig.12 ,like Fig.13 and Fig.14 shown.

[0065] Application Examples The application performance of the hollow mesoporous polymer material prepared in the present invention as a catalyst carrier is tested, and the effect of metal-carrier electronic interaction on the catalytic activity of benzaldehyde transfer hydrogenation is studied under different reaction temperatures, reaction times, hydrogen sources and other conditions.

[0066] The hollow structure mesoporous polyfurfuryl alcohol prepared in Example 3 was used as a carrier to load palladium nanoparticles to obtain a mesoporous polyfurfuryl alcohol-loaded palladium catalyst Pd / SCP-FA. The specific preparation method is as follows: (1) Add 20 mL of distilled water to a 250 mL volumetric flask. Add 188 µL of 0.1 mol / L chloropalladic acid (H2PdCl4) solution and 188 µL of 0.1 mol / L sodium citrate (Na3C6H5O7) solution at 800 rpm / min in an ice-water bath and stir for 10 min.

[0067] (2) Then, 1128 μL of 0.1 mol / L NaBH4 was added and the mixture was stirred for 8 min. After the reaction was completed, 0.2 g of hollow structure mesoporous polyfurfuryl alcohol SCP-FA was added and the mixture was stirred for 4 h under the same conditions.

[0068] (3) The reaction solution was then filtered and washed several times with distilled water and anhydrous ethanol. Finally, the obtained solid sample was freeze-dried to complete the preparation of the Pd / SCP-FA catalyst.

[0069] The same preparation method is adopted to respectively use the hollow structure mesoporous polypyrrole and hollow structure mesoporous polythiophene methanol prepared in Example 4 and 5 as carriers to load palladium nanoparticles to obtain mesoporous polypyrrole-supported palladium catalyst Pd / SCP-PY and mesoporous polythiophene methanol-supported palladium catalyst Pd / SCP-TPM.

[0070] The catalytic performance of the above-prepared mesoporous polyfurfuryl alcohol supported palladium catalyst Pd / SCP-FA, mesoporous polypyrrole supported palladium catalyst Pd / SCP-PY, and mesoporous polythiophene methanol supported palladium catalyst Pd / SCP-TPM in the transfer catalytic hydrogenation reaction of benzaldehyde compounds was tested, and the commercial catalyst Pd / C and the prepared homogeneous catalyst PdCl2 / SCP-TPM were used as comparative examples. The reaction formula and test method are as follows:

[0071] (1) Add 30 mg of catalyst to a 10 mL reaction tube, then add 0.5 mmol of benzaldehyde, 3 mL of isopropanol, and 20 mg of KOH to the reaction tube in sequence, and replace the gas in the reaction tube with nitrogen.

[0072] (2) After repeating the above operation 4 times, the reaction was continued at 50-80 °C for 3 h. After the reaction was completed, the mixture was diluted with ethyl acetate, and then the reactants and products were quantitatively analyzed by gas chromatography using 1,3,5-trimethoxybenzene as an internal standard. The test results are shown in Table 2 below: Table 2

[0073] It can be seen from Table 2 above: The catalyst prepared by using the mesoporous polymer material prepared in the present invention as a carrier to load palladium has good catalytic performance. In the transfer catalytic hydrogenation reaction of benzaldehyde compounds, the conversion rates of the mesoporous polypyrrole-loaded palladium catalyst Pd / SCP-PY and the mesoporous polythiophene methanol-loaded palladium catalyst Pd / SCP-TPM are significantly better than those of the commercial Pd / C.

[0074] Furthermore, the catalyst prepared by using the mesoporous polythiophene methanol as a carrier and supporting palladium provided in Example 5 has the best catalytic performance. Under the conditions of 80°C, normal pressure and isopropanol as a hydrogen source, it exhibits the best catalytic activity, and can achieve a benzaldehyde conversion rate of 98% and a product selectivity of 99%.

[0075] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a mesoporous polymer material based on organic-inorganic interaction at the porous silica interface, characterized in that: The following steps are involved: S1, mixing a polymer precursor with a solvent to obtain a precursor solution; the polymer precursor includes a combination of one or more of resol phenolic resin, furfuryl alcohol, 2-thiophene methanol, pyrrole, dopamine, thiophene, cyanamide, aniline, styrene, and pyridine; S2, dropping the precursor solution into the mesoporous silica template, and performing a first polymerization reaction at 25-150° C. to obtain a polymer / mesoporous silica composite; S3, placing the polymer / mesoporous silica composite at 200-480° C. for a second polymerization reaction; then etching the silica template, washing and drying the product to obtain a mesoporous polymer material with a hollow structure.

2. The preparation method according to claim 1, characterized in that: In step S1, the precursor solution also includes a catalyst; the catalyst includes one or more combinations of ferric chloride, oxalic acid, ferric nitrate, cupric chloride, cupric nitrate, ferric nitrate, ammonium persulfate, tin chloride, and aluminum chloride.

3. The preparation method according to claim 1, characterized in that: In step S1, the solvent includes one or more combinations of anhydrous ethanol, methanol, water, trimethylbenzene, ethylbenzene, n-hexane, N,N-dimethylformamide, dichloroethane, and 1,2-dichlorobenzene.

4. The preparation method according to claim 1, characterized in that: In step S2, the mesoporous silica template includes one or more combinations of SBA-15-OH, MCF-OH, KIT-6-OH, SBA-12-OH, FDU-12-OH and SBA-16-OH.

5. The preparation method according to claim 1, characterized in that When the polymer precursor is selected from one of resol phenolic resin, aniline, styrene, and dopamine, before step S3, the following operation is also included: mixing the polymer / mesoporous silica composite obtained in step S2 with a crosslinking agent and a catalyst, and performing a crosslinking reaction at 70-150° C. for 12-36 h to obtain a crosslinked polymer / mesoporous silica composite.

6. The preparation method according to claim 1, characterized in that: In step S3, the solvent used in the etching process includes one or more combinations of hydrofluoric acid, sodium hydroxide solution, and potassium hydroxide solution.

7. The preparation method according to claim 1, characterized in that In step S3, the drying process is performed by freeze drying, the freeze drying temperature is -90 to -40°C, and the freeze drying time is 1 to 48 hours.

8. A mesoporous polymer material based on organic-inorganic interaction at the porous silica interface, characterized in that: Prepared according to the preparation method described in any one of claims 1 to 7.

9. Use of the mesoporous polymer material based on organic-inorganic interaction at the porous silica interface according to claim 8 in catalysis, adsorption or biomedicine.

10. The use according to claim 9, characterized in that: The mesoporous polymer material is used as a carrier to load precious metals to prepare a catalyst, and the catalyst is applied to the transfer catalytic hydrogenation reaction of benzaldehyde compounds.