High-dispersity W18O49 / VO2 nano composite powder as well as low-temperature preparation method and application thereof
The highly dispersed W18O49/VO2 nanocomposite powder prepared by hydrothermal method solves the problems of uneven performance of VO2/W18O49 composite film and high thermal response temperature, and realizes the low-temperature phase transformation and thermal insulation performance of VO2 nanoparticles. In engineering applications, the film is waterproof and self-cleaning properties are given.
Patent Information
- Application Number
- CN202411193051.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing VO2/W18O49 composite diffusion film has uneven performance and high thermal response temperature, which affects its thermal insulation performance and reliability in practical applications.
The highly dispersed W18O49/VO2 nanocomposite powder was prepared by hydrothermal method. By mechanically stirring the granular VO2 and sheet-like W18O49 in a mixed solution of ethanol and polyethylene glycol, the size of W18O49 is controlled to be between 5nm and 15nm and 400nm± Within the range of 50 nm, and by oleic acid and oleamine as surfactants, the thermal response temperature of VO2 is reduced to 30°C to 40°C.
The phase transition response temperature reduction of VO2 nanoparticles is achieved, which improves the thermal insulation performance and application range, while reducing the energy consumption of the preparation process, provides a low-energy-consuming engineering application route, and gives the prepared film waterproof and Self-cleaning characteristics.
Smart Images

Figure CN119081235A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of functional films, and more specifically, relates to a W 18 O 49 / VO 2 Nanocomposite powder, preparation method and application thereof. Background Art
[0002] Energy depletion and environmental pollution have become two major problems that need to be solved urgently. Among them, building energy accounts for about 40% of the world's energy consumption, and up to 50% of building energy consumption is used to control indoor temperature. Therefore, how to reduce the energy required to control indoor temperature is the key to reducing building energy consumption.
[0003] Architectural glass is an extremely important component of building materials and one of the main materials for building energy consumption. Therefore, researchers at home and abroad have focused on developing more efficient and intelligent glass materials or optical films.
[0004] The key to the development of smart windows is that when the material is subjected to dynamic changes in the external environment, it can respond spontaneously or passively to achieve the desired effect. 2 ) is a typical thermochromic material, whose reversible metal-insulator transition is extremely fast and the temperature is 68℃, close to room temperature. Below the phase transition temperature, VO 2 It shows the insulating monoclinic M phase with high infrared transmittance, allowing more infrared light to pass through and increasing the indoor temperature. When the temperature is higher than the phase transition temperature, it shows the rutile R phase with low infrared transmittance, reducing infrared transmittance and lowering the indoor temperature. In this change process, the transmittance of visible light does not change much, and is only affected by the temperature response infrared automatic adjustment to let VO 2 The film keeps the room warm in winter and cool in summer.
[0005] In order to achieve VO 2 The practical application of thermochromic smart windows still has the following problems to be solved: 1. 2 The film has low light transparency, which affects normal indoor lighting. Its thermal insulation performance needs to be optimized and improved. Its phase transition temperature is 68°C, which is not suitable for actual applications. 2. Ordinary vanadium dioxide film does not have waterproof and self-cleaning properties. It is easily damaged and fallen off by wind and rain outdoors, and cannot meet the requirements of long-term outdoor use of the coating.
[0006] Patent application with application publication number CN115057625A discloses a composite diffused membrane and a preparation method, specifically a VO 2 / W 18 O 49 Composite diffuse film and preparation method thereof, wherein the film is composed of monoclinic vanadium dioxide nanoparticles, W 18 O 49The nanoparticles and the transparent film-forming agent polyvinyl pyrrolidone (PVP) are prepared by the following steps: 1) tungsten hexachloride (WCl 6 ) and anhydrous ethanol as raw materials for solvent thermal reaction to generate W 18 O 49 ; 2) W 18 O 49 The vanadium dioxide powder and PVP and ethanol were respectively ball-milled and mixed. The obtained solutions after ball milling were centrifuged and the supernatant was dried to obtain two coating powders. The two coating powders were mixed with ethanol in different mass ratios to prepare coating solutions. The coating solutions were evenly dropped on the glass substrate for spin coating. Although the preparation method is simple and the raw materials are simple, the prepared coating powder can be widely used in energy-saving glass and flexible energy-saving films in buildings. However, in actual research, it was found that the performance of the film was relatively uneven, the performance differences between different regions of the film were large, and the thermal response temperature was relatively high.
[0007] Therefore, it is necessary to develop a new type of VO with more uniform performance. 2 / W 18 O 49 Nanocomposite powders and films can be used in practical applications. Summary of the invention
[0008] In view of the defects of the prior art, the object of the present invention is to provide a 18 O 49 / VO 2 Nanocomposite powder, preparation method and application thereof, aiming to solve the existing VO 2 / W 18 O 49 The composite diffused membrane has uneven performance and the thermal response temperature is too high.
[0009] To achieve the above object, the first aspect of the present invention provides a highly dispersed W 18 O 49 / VO 2 Nanocomposite powder, which consists of granular VO 2 and lamellar W 18 O 49 The composite is prepared by mechanical stirring in a mixed solution of ethanol and polyethylene glycol according to a set mass ratio, wherein the lamellar W 18 O 49 The surface has oleic acid groups and oleylamine groups, which are used to make the lamellar W 18 O 49 The growth is hindered and the size is limited to a set range. The thickness of the sheet is 5nm to 15nm, the length of the sheet is 400nm ± 50nm, and the granular VO 2 The particle size is 40nm~80nm, granular VO2 Evenly dispersed in the lamellar W 18 O 49 surface.
[0010] According to a second aspect of the present invention, there is provided a method for preparing the highly dispersible W 18 O 49 / VO 2 The method of preparing nanocomposite powder adopts hydrothermal method throughout the process, which specifically includes the following steps:
[0011] S1: Preparation of VO by hydrothermal method 2 Nano powder,
[0012] S2: Preparation of W by hydrothermal method 18 O 19 Powder, specifically including the following sub-steps,
[0013] S21: Add oleic acid and oleylamine to anhydrous ethanol, stir and mix evenly to obtain a mixed solvent,
[0014] S22: Add tungsten chloride powder to the mixed solvent of step S21, and continue stirring until the blue-black tungsten chloride powder is completely dissolved to obtain a golden yellow and transparent solution.
[0015] S23: Rapidly transfer the golden yellow and transparent solution obtained in step S22 to a sealed container to prevent it from coming into contact with water vapor or being oxygenated, place the sealed container in a high-pressure reactor for hydrothermal reaction, and naturally cool to room temperature after the reaction to obtain a hydrothermal reaction product.
[0016] S24: The hydrothermal product obtained in step S23 is centrifugally washed with anhydrous ethanol and deionized water in sequence, then vacuum dried, and finally ground to obtain W 18 O 49 Nano flake powder,
[0017] Among them, step S1 and step S2 are in no particular order.
[0018] S3: VO 2 Nanopowder and W 18 O 19 Nano-flaky powder is compounded.
[0019] In the above hydrothermal method, W 18 O 19 During the process, oleic acid was added (the molecular formula of oleic acid is: CH 3 (CH 2 ) 7 CH=CH(CH 2 ) 7 COOH) and oleylamine (the molecular formula of oleylamine is: C 18 H37 N), oleic acid and oleylamine are used as surfactants, which can change the morphology of nanoparticles and present a flaky structure. If oleic acid and oleylamine are not added as surfactants, the hydrothermal method is used to prepare W 18 O 19 In the process, W 18 O 19 Tends to grow into large granules, resembling a sea urchin in appearance.
[0020] Furthermore, in step S21, the volume ratio of anhydrous ethanol to oleic acid and oleylamine is 80:3 to 80:5, and in step S22, the mass ratio of oleic acid to tungsten chloride powder is 0.9:0.2 to 0.9:0.4.
[0021] Furthermore, in step S23, the temperature of the hydrothermal reaction is 160-190° C., and the time of the hydrothermal reaction is 22-26 hours.
[0022] Further, in step S1, VO is prepared 2 The specific steps of nano powder are:
[0023] S11: Dissolve ammonium metavanadate in deionized water and stir evenly to obtain a milky white ammonium salt suspension.
[0024] S12: Dissolve the reducing agent hydrazine monohydrochloride in water and stir until completely dissolved. Then add the milky white ammonium salt suspension dropwise. The solution first turns gray-black and then brown-yellow. Continue stirring and add concentrated hydrochloric acid dropwise. The solution slowly turns from brown-yellow to gray-green and then to a blue clear solution. Keep stirring.
[0025] S13: using ammonia water as a precipitant, adding the blue clear solution dropwise, the blue clear solution gradually changes to brownish yellow earth color, adjusting its pH, continuing to stir, obtaining a precipitate, and washing the precipitate by centrifugation.
[0026] S14: The brown-yellow earth-colored precipitate washed by centrifugation is transferred to the inner tank of the reactor, and an appropriate amount of ultrapure water is added to obtain a precursor. The volume of the precursor is adjusted to, for example, 80% of the volume of the polytetrafluoroethylene liner. After ultrasonication for, for example, 30 minutes, the PPL liner (polytetrafluoroethylene) is placed in the metal reactor for hydrothermal reaction.
[0027] S15: The hydrothermal reaction product was centrifuged and washed twice with deionized water, ethanol and isopropanol, and then vacuum dried and fully ground to obtain VO 2 Powder, VO 2 The powder particle size is 40 to 80 nm.
[0028] Furthermore, in step S13, the pH is adjusted to 8-8.6, and in step S14, the temperature of the hydrothermal reaction is 260-290° C., and the time of the hydrothermal reaction is 22-26 hours.
[0029] Further, in step S3, VO 2 Nanopowder and W 18 O 19 The specific steps of compounding nano-flaky powders are:
[0030] The VO obtained in step S1 is 2 Nanopowder and step S2 to obtain W 18 O 49 The nano-flaky powder is added to a mixed solution of ethanol and polyethylene glycol in a mass ratio of 4:1 to 1:1 and mechanically stirred. In the mixed solution of ethanol and polyethylene glycol, the mass ratio of ethanol and polyethylene glycol is 50:3 to 50:5. After the stirring is completed, the product is washed and dried, and then ground to obtain W 18 O 49 / VO 2 Composite powder.
[0031] In the above invention, the first step is to synthesize a high solar light regulation capacity (T sol ) 2 Powder, then hydrothermally prepared with high infrared shielding ability W 18 O 49 Nano powder.
[0032] In the above invention, the long chain part of oleylamine will dissolve in ethanol. At this time, the double bonds of the long chain will cause the spatial structure to bend more violently, and then generate a larger spatial barrier, providing a greater repulsive force, so that the lamellar W 18 O 49 The twisting produces stacking, making the lamellar structure more obvious. Oleic acid controls W 18 O 49 The crystals grow because oleic acid reduces W when it participates in the hydrothermal reaction. 18 O 49 The growth of the crystal is controlled along the (010) crystal plane. The combination of oleic acid and oleylamine can control the size of tungsten oxide within a certain range. The specific size range is 400nm±50nm in length and 5-15nm in thickness. 18 O 49 and VO 2 The hydrothermal method was used to compound VO 2 The thermal response temperature of the composite vanadium dioxide has a good control effect, which reduces its thermal response temperature from the phase transition temperature of 68°C to 30°C~40°C. The thermal response temperature is different from the phase transition temperature. The phase transition temperature refers to the phase transition temperature of the vanadium dioxide powder, and the thermal response temperature refers to the temperature of the composite vanadium dioxide in W 18 O 49 The ambient temperature is the temperature at which vanadium dioxide absorbs a certain amount of heat under the action of the vanadium dioxide phase change.
[0033] In fact, the improvement of the thermal insulation ability of the composite powder under long-term infrared irradiation is due to the introduction of W with high transmittance and high infrared shielding ability. 18 O 49 More importantly, W 18 O 49 The particle size specification deviation is small, which can maximize the effectiveness. Under the condition of short-term infrared irradiation, its heat insulation capacity is improved to a greater extent, which proves that the introduction of particle size specification deviation is small. 18 O 49 Finally, by utilizing its excellent photothermal conversion efficiency, VO can be stimulated more quickly. 2 Nanoparticles undergo phase transformation and play a heat-insulating role, which is to reduce VO 2 Nanoparticle phase transitions in response to temperature, extending VO 2 This is an effective means of nanomaterial application. This has been disclosed in the existing literature, but the present invention further optimizes W based on the existing literature. 18 O 49 The effect of synthesizing W with size and morphology limited to a specific range 18 O 49 , and VO 2 The distribution is more ideal, which ultimately enables it to stimulate VO faster 2 Nanoparticles undergo phase transition and have a lower thermal response temperature, which can actually play their thermal insulation role.
[0034] According to a third aspect of the present invention, there is also provided a highly dispersible W 18 O 49 / VO 2 The application of nanocomposite powder is used to prepare thermochromic temperature-control film.
[0035] Furthermore, FEVE fluorocarbon resin (full name: polytrifluorochloroethylene / vinyl ether resin) is mixed with high dispersibility W 18 O 49 / VO 2 Nanocomposite powders for the preparation of thermochromic temperature-controlling films with high dispersion W 18 O 49 / VO 2 The mass ratio of nanocomposite powder to FEVE resin is 0.1:5 to 0.2:5, and the thermal response temperature of the obtained color-changing temperature-control film is 30°C to 40°C. FEVE resin has the properties of waterproof, self-cleaning and corrosion-resistant, which can make the obtained thermochromic temperature-control film waterproof and weather-resistant.
[0036] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0037] 1. W in the present invention 18 O 49 / VO 2 In nanocomposite powder, W 18 O 49 The surface has oleic acid groups and oleylamine groups, which are used to make the lamellar W 18 O 49 Growth is hindered and the size is limited to a set range, specifically the sheet thickness is 5nm to 15nm, the sheet length is 400nm ± 50nm, its morphology and size specifications are relatively regular with small deviations and good consistency, which can maximize the stimulation of VO 2 Nanoparticles undergo phase transformation, reducing VO 2 Nanoparticles phase transition in response to temperature, play their role in heat insulation, is the key to expand VO 2 Nanomaterials are an effective means of application, specifically, they can convert VO 2 The phase transition response temperature of nanoparticles drops from 68℃ to 30℃~40℃ (that is, when the ambient temperature is 30℃~40℃, VO 2 Nanoparticles can undergo phase change without waiting for a higher ambient temperature, such as 68°C or above 50°C, and can be effectively applied in engineering practice.
[0038] 2. The present invention prepares W by hydrothermal method throughout the process 18 O 49 / VO 2 Nanocomposite powders do not require high temperatures throughout the entire process, the preparation temperature is moderate, the process is simple and easy, and the energy consumption in the preparation process is reduced. This changes the preparation conditions that require high costs and high precision to improve performance, and provides a low-energy process route that can be effectively applied in engineering.
[0039] 3. The present invention adopts W 18 O 49 / VO 2 -KH570 composite film structure, which has the characteristics of waterproofing and temperature control, is conducive to the further introduction of other functional films. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is W obtained by different preparation methods in this embodiment 18 O 19 Nanopowder, among which Figure 1 In the content, (a) is W prepared in Example 5 18 O 19 Nano powder, Figure 1 In the content, (b) is W prepared in Example 6 18 O 19 Nano powder, Figure 1 In the content, (c) is W prepared in Example 7 18 O 19 Nano powder, Figure 1 In the content, (d) is W prepared in Example 1 18 O 19 Nano powder.
[0041] Figure 2 W prepared in Example 1 18 O 19 Nano powder, W prepared in Example 5 18 O 19 Nanopowder, W prepared in Example 6 18 O 19 Nanopowder, W prepared in Example 7 18 O 19 XRD and FTIR spectra of nanopowders, Figure 2 Content (a) refers to the preparation of W in Example 1, Example 5, Example 6 and Example 7, respectively. 18 O 19 XRD pattern of nanopowder, Figure 2 Content (b) refers to the preparation of W in Example 1, Example 5, Example 6 and Example 7, respectively. 18 O 19 FTIR spectrum of nanopowder.
[0042] Figure 3 W is prepared by step 3 of Example 1 18 O 49 / VO 2 XRD patterns of composite powders.
[0043] Figure 4 W is prepared by step 3 of Example 1 18 O 49 / VO 2 SEM images of the composite powder and corresponding O, V and W element mapping images.
[0044] Figure 5 The multilayer W obtained in Example 8 18 O 49 / VO 2 Actual picture of the large glass prepared by thin film.
[0045] Figure 6 Graph showing the optical properties of the product obtained in Example 9, wherein the solid line indicates the transmittance curve of the film at 20°C, the dotted line indicates the transmittance curve of the film at 90°C, S1 indicates coating of one layer of film, S2 indicates coating of two layers of film, and S3 indicates coating of three layers of film. Figure 6 Three Ws are given in 18 O49 / VO 2 The visible light transmittance of the intelligent waterproof temperature control film gradually decreases. The visible light transmittance of S1 is T 550nm =58.3%, the visible light transmittance of S2 is T 550nm =44.1%, the visible light transmittance of S3 is T 550nm =33.6%. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0047] The phrases "one embodiment", "one example" or similar language of this specification indicate that a particular feature, structure or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present invention. Therefore, the phrases "in one embodiment" and similar language may, but do not necessarily, all refer to the same embodiment.
[0048] Example 1
[0049] The present invention provides a W 18 O 49 / VO 2 A method for preparing a composite material, in one embodiment, the method comprises the following steps:
[0050] Step 1: Highly dispersed VO 2 Preparation of nanopowders:
[0051] (1) Dissolve the ammonium salt in deionized water, place in a heated magnetic stirrer, and stir evenly to obtain a milky white mixed solution. The heated magnetic stirrer is adjusted at a temperature of 30° C. and a rotation speed of 1500 r / min.
[0052] (2) Dissolve the reducing agent in water and stir until completely dissolved. Add the ammonium salt suspension dropwise. Observe that the suspension turns gray-black and finally brown-yellow. Continue stirring.
[0053] (3) The beaker was transferred to a fume hood, and concentrated hydrochloric acid was taken with a pipette under vigorous stirring. The concentration of the concentrated hydrochloric acid was 99 wt %. The solution was added dropwise. The reaction was vigorous and the color of the mixed solution slowly changed from brown to gray-green with a large number of bubbles generated until the mixed solution became a clear blue solution. The mixture was stirred.
[0054] (4) Ammonia water was used as a precipitant and added dropwise. The clear blue solution gradually changed to brownish yellow earth color. The pH value was adjusted to 8.6. Stirring was continued and the solution was washed by centrifugation with deionized water. The speed of the centrifuge was adjusted to 6000 r / min for 5 min.
[0055] (5) The brown-yellow earthy precipitate is transferred to the inner liner of the reactor, and an appropriate amount of ultrapure water is added to obtain a precursor. The volume of the precursor is adjusted to 80% of the volume of the PPL lining. After ultrasonic treatment for 30 minutes, the PPL lining is placed in a metal reactor for hydrothermal treatment at a temperature of 270°C for 1440 minutes (24 hours).
[0056] (6) The black reaction product obtained in step 5) was centrifuged and washed twice with deionized water, ethanol and isopropanol, and then vacuum dried and fully ground to obtain VO 2 Powder.
[0057] The VO prepared in this step 2 The average particle size of the nanoparticles is 40 to 80 nm.
[0058] Step 2, W 18 O 19 Preparation of nanopowders.
[0059] (1) Take anhydrous ethanol in a blue-capped bottle, add appropriate amounts of surfactants oleic acid and oleylamine, stir to mix the solvents evenly for later use, and the volume ratio of anhydrous ethanol to oleic acid and oleylamine is 80:3;
[0060] (2) Place the blue-capped bottle in a glove box and continue stirring. Weigh tungsten chloride powder in the glove box and transfer it to the above mixed solution. The mass ratio of oleic acid to oleylamine to tungsten chloride powder is 0.9:0.2. Continue stirring in the glove box for about 10 minutes until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0061] (3) Take out the blue-capped bottle from the glove box and quickly transfer the yellow transparent solution to the polytetrafluoroethylene liner (to prevent the yellow solution from being oxidized by water vapor and oxygen);
[0062] (4) The polytetrafluoroethylene liner was placed in a high-pressure reactor for hydrothermal treatment at a temperature of 180°C for 24 hours. After the reaction was completed, the liner was naturally cooled to room temperature and taken out. The liner was centrifuged and washed four times with anhydrous ethanol and deionized water, and then vacuum dried at a temperature of 80°C for 6 hours. After grinding, W was obtained. 18 O 49 Nano powder.
[0063] In this step, W is prepared hydrothermally 18 O 49 Adding an appropriate amount of surfactant (oleic acid and oleylamine) in the process of nanopowder can change the morphology of nanoparticles, showing a flake-like and stacked multilayer structure. 18 O 49 The length of nanopowder is in the range of 350nm to 450nm, and the thickness is approximately 5nm to 15nm.
[0064] Step 3, W 18 O 49 / VO 2 Preparation of composite powder
[0065] (1) Change VO 2 Powder and W 18 O 49 The powder is mechanically stirred and compounded in 50 ml of anhydrous ethanol and PEG-2000 (polyethylene glycol) solution according to a certain mass ratio. The stirring and compounding is completed. 2 Nanopowder and W 18 O 49 The nano-flaky powder was added into a mixed solution of ethanol and polyethylene glycol at a mass ratio of 4:1 and mechanically stirred. In the mixed solution of ethanol and polyethylene glycol, the mass ratio of ethanol and polyethylene glycol was 50:3.
[0066] (2) The product was washed three times by centrifugation with deionized water and ethanol, vacuum dried and fully ground. The vacuum drying temperature was 80°C and the vacuum drying time was 6 h to obtain W. 18 O 49 / VO 2 Composite powder.
[0067] Example 2
[0068] This embodiment is basically the same as embodiment 1, except that the process parameters of some key steps are different. The changes of some key process parameters are listed below:
[0069] Step 1: Highly dispersed VO 2 Preparation of nanopowders:
[0070] (4) Ammonia water was used as a precipitant and added dropwise. The clear blue solution gradually changed to brownish yellow earth color. The pH value was adjusted to 8. Stirring was continued and the solution was washed by centrifugation with deionized water. The speed of the centrifuge was adjusted to 5500 r / min for 9 min.
[0071] (5) The brown-yellow earthy precipitate was transferred to the inner tank of the reactor, and an appropriate amount of ultrapure water was added to obtain a precursor. The volume of the precursor was adjusted to 80% of the volume of the PPL lining. After ultrasonic treatment for 30 minutes, the PPL lining was placed in a metal reactor for hydrothermal treatment at a temperature of 290°C for 22 hours.
[0072] The VO prepared in this step 2 The average particle size of the nanoparticles is 60 to 80 nm.
[0073] Step 2, W 18 O 19 Preparation of nanopowders.
[0074] (1) Take anhydrous ethanol in a blue-capped bottle, add appropriate amounts of surfactants oleic acid and oleylamine, stir to mix the solvents evenly for later use, and the volume ratio of anhydrous ethanol to oleic acid and oleylamine is 80:5;
[0075] (2) Place the blue-capped bottle in a glove box and continue stirring. Weigh tungsten chloride powder in the glove box and transfer it to the above mixed solution. The mass ratio of oleic acid to oleylamine and tungsten chloride powder is 0.9:0.4. Continue stirring in the glove box for about 10 minutes until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0076] (4) The polytetrafluoroethylene liner was placed in a high-pressure reactor for hydrothermal treatment at a temperature of 160°C for 26 hours. After the reaction was completed, the liner was naturally cooled to room temperature and taken out. The liner was centrifuged and washed four times with anhydrous ethanol and deionized water, and then vacuum dried at a temperature of 75°C for 7 hours. After grinding, W was obtained. 18 O 49 Nano powder.
[0077] In this step, W is prepared hydrothermally 18 O 49 Adding an appropriate amount of surfactant (oleic acid and oleylamine) in the process of nanopowder can change the morphology of nanoparticles, showing a flake-like and stacked multilayer structure. 18 O 49 The length of the nanopowder is in the range of 370nm to 440nm, and the thickness is approximately 5nm to 15nm.
[0078] Step 3, W 18 O 49 / VO 2 Preparation of composite powder
[0079] (1) Change VO 2 Powder and W 18 O 49 The powder is mechanically stirred and compounded in 50 ml of anhydrous ethanol and PEG-2000 (polyethylene glycol) solution according to a certain mass ratio. The stirring and compounding is completed. 2 Nanopowder and W 18 O 49 The nano-flaky powder was added into a mixed solution of ethanol and polyethylene glycol at a mass ratio of 1:1 and mechanically stirred. In the mixed solution of ethanol and polyethylene glycol, the mass ratio of ethanol and polyethylene glycol was 50:5.
[0080] (2) The product was washed three times by centrifugation with deionized water and ethanol, vacuum dried and fully ground. The vacuum drying temperature was 85°C and the vacuum drying time was 5.5 h to obtain W. 18 O 49 / VO 2Composite powder.
[0081] Example 3
[0082] This embodiment is basically the same as embodiment 1, except that the process parameters of some key steps are different. The changes of some key process parameters are listed below:
[0083] Step 1: Highly dispersed VO 2 Preparation of nanopowders:
[0084] (4) Ammonia water was added dropwise as a precipitant, and the clear blue solution gradually changed to brownish yellow earth color. The pH value was adjusted to 8.2, and stirring was continued. The solution was washed by centrifugation with deionized water. The speed of the centrifuge was adjusted to 6500 r / min for 5 min.
[0085] (5) The brown-yellow earthy precipitate was transferred to the inner tank of the reactor, and an appropriate amount of ultrapure water was added to obtain a precursor. The volume of the precursor was adjusted to 80% of the volume of the PPL lining. After ultrasonic treatment for 30 minutes, the PPL lining was placed in a metal reactor for hydrothermal treatment at a temperature of 260°C for 26 hours.
[0086] The VO prepared in this step 2 The average particle size of the nanoparticles is 40 to 65 nm.
[0087] Step 2, W 18 O 19 Preparation of nanopowders.
[0088] (1) Take anhydrous ethanol in a blue-capped bottle, add appropriate amounts of surfactants oleic acid and oleylamine, stir to mix the solvents evenly for later use, and the volume ratio of anhydrous ethanol to oleic acid and oleylamine is 80:4;
[0089] (2) Place the blue-capped bottle in a glove box and continue stirring. Weigh tungsten chloride powder in the glove box and transfer it to the above mixed solution. The mass ratio of oleic acid to oleylamine to tungsten chloride powder is 0.9:0.3. Continue stirring in the glove box for about 10 minutes until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0090] (4) The polytetrafluoroethylene liner was placed in a high-pressure reactor for hydrothermal treatment at a temperature of 190°C for 22 hours. After the reaction was completed, the liner was naturally cooled to room temperature and taken out. The liner was centrifuged and washed four times with anhydrous ethanol and deionized water, and then vacuum dried at a temperature of 80°C for 6 hours. After grinding, W was obtained. 18 O 49 Nano powder.
[0091] In this step, W is prepared hydrothermally 18 O 49Adding an appropriate amount of surfactant (oleic acid and oleylamine) in the process of nanopowder can change the morphology of nanoparticles, showing a flake-like and stacked multilayer structure. 18 O 49 The length of nanopowder is in the range of 360nm to 450nm, and the thickness is approximately 5nm to 15nm.
[0092] Step 3, W 18 O 49 / VO 2 Preparation of composite powder
[0093] (1) Change VO 2 Powder and W 18 O 49 The powder is mechanically stirred and compounded in 50 ml of anhydrous ethanol and PEG-2000 (polyethylene glycol) solution according to a certain mass ratio. The stirring and compounding is completed. 2 Nanopowder and W 18 O 49 The nano-flaky powder was added into a mixed solution of ethanol and polyethylene glycol at a mass ratio of 3:1 and mechanically stirred. In the mixed solution of ethanol and polyethylene glycol, the mass ratio of ethanol and polyethylene glycol was 50:4.
[0094] (2) The product was washed three times by centrifugation with deionized water and ethanol, vacuum dried and fully ground. The vacuum drying temperature was 80°C and the vacuum drying time was 6 h to obtain W. 18 O 49 / VO 2 Composite powder.
[0095] Example 4
[0096] Example 4 is a comparative example relative to Example 1, except that the polyethylene glycol in step (1) of step 3 is removed on the basis of Example 1.
[0097] The process and parameters of this embodiment are the same as those of embodiment 1, the only difference being:
[0098] Step 3, W 18 O 49 / VO 2 Preparation of composite powder
[0099] (1) Change VO 2 Powder and W 18 O 49 The powders are mechanically stirred and compounded in 50 ml of anhydrous ethanol solution according to a certain mass ratio.
[0100] Test experiment: Through SEM scanning of Example 1 and Example 4, it can be seen that the addition of polyethylene glycol increases the steric hindrance between the nanoparticles and improves the dispersibility of the nanoparticles.2 In W 18 O 49 The surface dispersion is more uniform and there is no agglomeration.
[0101] Example 5
[0102] This example is a comparative example of step 2 in Example 1. 18 O 19 When the nano powder was prepared, no surfactants, oleic acid and oleylamine, were added. 18 O 19 The preparation of nanopowders is as follows:
[0103] (1) Take 80 ml of anhydrous ethanol in a 250 ml blue-capped bottle, put the blue-capped bottle into a glove box, weigh 0.8 g of tungsten chloride powder in the glove box and transfer it to the above mixed solution, and continue to stir in the glove box for about 15 minutes until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0104] (2) Take out the blue-cap bottle from the glove box, quickly transfer the yellow transparent solution to a 100 ml polytetrafluoroethylene liner (to prevent the yellow solution from being oxidized by water vapor and oxygen), then place the polytetrafluoroethylene liner in a high-pressure reactor, perform a hydrothermal reaction at 180°C for 24 hours, cool naturally to room temperature after the reaction, wash with anhydrous ethanol and deionized water for 4 times by centrifugation, and then dry at 80°C for 6 hours. After grinding, W 18 O 49 Nano powder.
[0105] Example 6
[0106] This example is a comparative example of step 2 in Example 1. 18 O 19 When nano powder, only surfactant oleic acid was added. 18 O 19 The preparation of nanopowders is as follows:
[0107] (1) Take 80 ml of anhydrous ethanol in a 250 ml blue-capped bottle, add 4 ml of oleic acid, and stir for 30 min to mix the solvent evenly for use; put the blue-capped bottle into a glove box and continue stirring, weigh 0.8 g of tungsten chloride powder in the glove box and transfer it to the above mixed solution, and continue stirring in the glove box for about 15 min until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0108] (2) Take out the blue-cap bottle from the glove box, quickly transfer the yellow transparent solution to a 100 ml polytetrafluoroethylene liner (to prevent the yellow solution from being oxidized by water vapor and oxygen), then place the polytetrafluoroethylene liner in a high-pressure reactor, perform a hydrothermal reaction at 180°C for 24 hours, cool naturally to room temperature after the reaction, wash with anhydrous ethanol and deionized water for 4 times by centrifugation, and then dry at 80°C for 6 hours. After grinding, W 18 O 49 Nano powder.
[0109] Example 7
[0110] This example is a comparative example of step 2 in Example 1. 18 O 19 When the nanopowder was prepared, only the surfactant CTAB (Chinese name: hexadecyl trimethyl ammonium bromide) was added. 18 O 19 The preparation of nanopowders is as follows:
[0111] (1) Take 80 ml of anhydrous ethanol in a 250 ml blue-capped bottle, add 1 g of CTAB (Chinese abbreviation: hexadecyltrimethylammonium bromide), and stir for 30 minutes to mix the solvent evenly for use; put the blue-capped bottle into a glove box and continue stirring, weigh 0.8 g of tungsten chloride powder in the glove box and transfer it to the above mixed solution, and continue stirring in the glove box for about 15 minutes until the blue-black tungsten chloride powder is completely dissolved to obtain a golden and transparent solution.
[0112] (2) Take out the blue-cap bottle from the glove box, quickly transfer the yellow transparent solution to a 100 ml polytetrafluoroethylene liner (to prevent the yellow solution from being oxidized by water vapor and oxygen), then place the polytetrafluoroethylene liner in a high-pressure reactor, perform a hydrothermal reaction at 180°C for 24 hours, cool naturally to room temperature after the reaction, wash with anhydrous ethanol and deionized water for 4 times by centrifugation, and then dry at 80°C for 6 hours. After grinding, W 18 O 49 Nano powder.
[0113] Detection experiment: W prepared in Example 1 18 O 19 Nano powder, W prepared in Example 5 18 O 19 Nanopowder, W prepared in Example 6 18 O 19 Nanopowder, W prepared in Example 7 18 O 19 The nanopowders were subjected to scanning electron microscope to observe their morphology. Figure 1 As shown, Figure 1 W obtained by different preparation methods18 O 19 Nano powder, Figure 1 In the content, (a) is W prepared in Example 5 18 O 19 Nano powder, Figure 1 In the content, (b) is W prepared in Example 6 18 O 19 Nano powder, Figure 1 In the content, (c) is W prepared in Example 7 18 O 19 Nano powder, Figure 1 In the content, (d) is W prepared in Example 1 18 O 19 Nanopowder. Example 5 presents a "sea urchin-like" structure, which is a spherical particle with a large number of spikes on the surface. The particle size of a single "sea urchin" is about 800nm, indicating that the W prepared without the action of a surfactant 18 O 19 The nanopowders did not present a lamellar shape. The W prepared in Example 6 (adding only oleic acid) and Example 7 (adding only CTAB) 18 O 19 Nano powders are 500nm to 700nm, and the powder particle size is similar to particles or elongated particles, which is a transition to lamellar. The average particle size of Example 1 (adding oleic acid and oleylamine at the same time) is 400nm, and the elongated particles are connected end to end to form long lamellar structures. It can be seen that: 1) when the cationic surfactant CTAB (hexadecyltrimethylammonium bromide) is added, the resulting sample tends to grow into a lamellar structure. When the surfactants are oleic acid and oleylamine, this lamellar structure is more obvious. 18 O 49 During the nucleation process, oleic acid and oleylamine are adsorbed on different surfaces of the nucleus. The polar group -NH 2 Coordination with W ions will also affect the polymerization of W ions, and like CTAB, it will reduce W 18 O 49 The trend of forming one-dimensional nanowires is developing towards two-dimensional nanosheet structures.
[0114] Figure 2 W prepared in Example 1 18 O 19 Nano powder, W prepared in Example 5 18 O 19 Nanopowder, W prepared in Example 6 18 O 19 Nanopowder, W prepared in Example 7 18 O 19 XRD and FTIR spectra of nanopowders, Figure 2Content (a) refers to the preparation of W in Example 1, Example 5, Example 6 and Example 7, respectively. 18 O 19 The XRD patterns of the nanopowders show that the powders prepared under the action of the three surfactants have characteristic diffraction peaks at 2θ=23.2°, 26.24°, 34.56° and 47.51°, which correspond to the monoclinic W 18 O 49 The (010), (210), (204) and (504) crystal planes of W were found to be consistent with the results reported in the relevant literature, and no other impurity peaks appeared. It can be seen that the surfactant does not participate in the reaction process and only affects the specific surface area and morphology of the synthesized sample. In addition, it was found that the diffraction peaks of the product obtained by adding oleic acid and oleylamine during the hydrothermal reaction were the strongest and sharpest, indicating that the addition of surfactants during the synthesis process has an important effect on the W 18 O 49 The intensity of the crystal diffraction peak has a certain influence. Figure 2 Content (b) refers to the preparation of W in Example 1, Example 5, Example 6 and Example 7, respectively. 18 O 19 FTIR spectrum of nanopowder. It can be seen from the figure that the absorption peaks of the powder added with surfactant during the hydrothermal process appear at 551cm -1 、1620cm -1 、2861cm -1 、2930cm -1 and 3426cm -1 Nearby. 551cm -1 Corresponding to W 18 O 49 The stretching vibration absorption peak of WO; 1620cm -1 and 3426cm -1 The corresponding absorption peaks are the antisymmetric stretching vibration and bending vibration absorption peaks of the OH group. The reason for the existence of these two characteristic peaks of the OH group is that the surface of the nanoparticles may contain a large number of hydroxyl groups; at 2930cm -1 and 2861cm -1 There are absorption peaks at , which correspond to the methylene groups (CH 2) Symmetric and asymmetric CH stretching vibrations in the W 18 O 19 The powder does not have the CH stretching vibration peak of the methylene group. From the XRD and infrared spectra, it can be preliminarily determined that the prepared nanopowder is W 18 O 49 , and no other impurities are generated.
[0115] Figure 3 W is prepared by step 3 of Example 1 18 O49 / VO 2 XRD spectrum of composite powder. It can be seen from the figure that the preparation process of composite powder will not change W 18 O 49 Powder and VO 2 The obtained phase composition of the powders is consistent, and both types of powders can exert their functional properties, which shows that the composite powders are successfully prepared from a qualitative point of view.
[0116] Figure 4 W is prepared by step 3 of Example 1 18 O 49 / VO 2 The SEM spectrum of the composite powder and the corresponding O, V and W element mapping spectrum. It can be seen from the figure that particles can be observed on the surface in the gray scanning electron micrograph, which are distributed on the W 18 O 49 Surface VO 2 From the O, V and W element mapping, it can be observed that the V and W elements are distributed evenly, indicating that VO 2 Most of the nanoparticles are loaded on W 18 O 49 There is no VO on the sheet. 2 The situation of gathering together alone is beneficial to W 18 O 49 Absorbs near-infrared light to stimulate VO more directly and quickly 2 Phase transformation occurs, which better realizes its function. It also explains that the composite powder W 18 O 49 / VO 2 Successful preparation.
[0117] Example 8
[0118] Using the W prepared above 18 O 49 / VO 2 Composite powder can be prepared 18 O 49 / VO 2 Composite coating, the specific method is as follows:
[0119] (1) The W obtained in step 3 18 O 49 / VO 2 The composite powder, PVP and anhydrous ethanol were added into the reagent bottle in the ratio of 1g:1g:40mL, and 1mm ball milling beads were added to cover the bottom of the reagent bottle. The mixture was stirred at room temperature to obtain a uniformly dispersed W 18 O 49 / VO 2The slurry was stirred at a speed of 2000 r / min and stirred for 24 h.
[0120] (2) The slurry obtained in step (1) was allowed to stand for 12 hours to allow large particles to settle, and only the slurry with uniform dispersion on the upper layer was selected.
[0121] (3) Use a pipette to weigh 200 μL of VO 2 The supernatant of the slurry or composite powder slurry is evenly dripped onto the treated glass substrate, and the intelligent temperature control coating is prepared by spin coating using a compact spin coater. The spin coating parameters are: low speed 900r / min, acceleration 400r / min 2 , time is 12s, high speed is 1800r / min, acceleration is 600r / min 2 , time is 20s.
[0122] (4) Place the spin-coated glass substrate on a heating plate to accelerate the volatilization of anhydrous ethanol. Adjust the temperature of the heating plate to 60°C and dry for 1 min. Repeat the above steps 2 to 3 times to obtain a multilayer W 18 O 49 / VO 2 film.
[0123] Figure 5 The multilayer W obtained in Example 8 18 O 49 / VO 2 The actual picture of the large glass prepared with the film shows that it is visible to the naked eye, with a lighter color, better transparency, and a uniform and glossy surface.
[0124] Example 9
[0125] Using the W prepared above 18 O 49 / VO 2 The composite powder can be used to prepare a waterproof intelligent temperature-control film. The specific method is as follows:
[0126] (1) Place 20 ml of ethanol and water in a three-necked flask, adjust the pH to 3-5 with hydrochloric acid, and heat in an oil bath with stirring.
[0127] (2) Add 0.2 g KH570 dropwise into the three-necked flask described in step (1), and continue heating and stirring in an oil bath.
[0128] (3) Dispersed W 18 O 49 / VO 2 The composite powder solution was added dropwise to the three-necked flask described in step (2), heated and stirred for 3 h, centrifuged and washed, and vacuum dried to obtain the modified W 18 O 49 / VO 2-KH570 powder. Use silane coupling agent to give W 18 O 49 / VO 2 The surface grafting modification of composite powder can reduce the agglomeration of nanoparticles and enable better dispersion in the resin.
[0129] (4) Add the powder obtained in step (3) and FEVE resin into a reagent bottle, and the high dispersibility W 18 O 49 / VO 2 The mass ratio of nanocomposite powder to fluorocarbon resin was 0.1:5. 1 mm ball milling beads were added to cover the bottom of the reagent bottle and stirred at room temperature to obtain a uniformly dispersed W 18 O 49 / VO 2 -Resin slurry of KH570.
[0130] (5) After standing, only the slurry with uniform dispersion on the upper layer is selected, and the supernatant is weighed with a pipette and evenly added to the treated glass substrate. The intelligent temperature control coating is prepared by spin coating using a compact spin coater. The spin coating parameters are: low speed 900 r / min, acceleration 400 r / min 2 , time is 12s, high speed is 1800r / min, acceleration is 600r / min 2 , time is 20s. Place the spin-coated glass substrate on a heating plate to accelerate the volatilization of anhydrous ethanol, adjust the temperature of the heating plate to 60℃, and dry for 1min. Repeat the above steps 2 to 3 times to obtain a multilayer W 18 O 49 / VO 2 Intelligent waterproof and temperature-control film.
[0131] Adhesion test and water resistance test were carried out on the above waterproof intelligent temperature control film. The film had excellent adhesion, which was grade 0 in ISO grade. After being immersed in 3.5% saline for 28 days, the surface of the film began to lose color, but there was almost no loss of gloss, bubbles or wrinkles, indicating that the film has excellent waterproof performance.
[0132] Figure 6 Graph showing the optical properties of the product obtained in Example 9, wherein the solid line indicates the transmittance curve of the film at 20°C, the dotted line indicates the transmittance curve of the film at 90°C, S1 indicates coating of one layer of film, S2 indicates coating of two layers of film, and S3 indicates coating of three layers of film. Figure 6 Three Ws are given in 18 O 49 / VO 2 The visible light transmittance of the intelligent waterproof temperature control film gradually decreases. The visible light transmittance of S1 is T 550nm =58.3%, the visible light transmittance of S2 is T 550nm=44.1%, the visible light transmittance of S3 is T 550nm = 33.6%, considering both the sunlight regulation capability and visible light transmittance, S2 has the best performance. 18 O 49 / VO 2 Optical properties of composite powder intelligent temperature control coating compared with W before modification 18 O 49 / VO 2 -Optical performance of PVP is reduced by only 20%.
[0133] The slurry prepared by the product obtained in this example was coated on a large glass to simulate actual use. The thickness of the intelligent temperature control film was about 20 μm, and compared with blank glass and pure VO 2 Comparative test of intelligent temperature control film. The experimental results show that when irradiated with near-infrared light for 60 seconds, the film of this embodiment has a heat insulation capacity of 10.4℃ higher than that of blank glass and higher than that of pure VO 2 The 9.2℃ of the intelligent temperature control film is 13% higher; when irradiated with near-infrared light for 480s, the composite powder film has a heat insulation capacity of 17.4℃ higher than that of blank glass and higher than that of pure VO 2 The intelligent temperature control film is 16.0℃ higher than 8.75%. Further analysis shows that: the introduction of W with uniform particle size 18 O 49 , using its excellent photothermal conversion efficiency, can stimulate VO faster 2 The nanoparticles undergo phase transition, and their thermal response temperature is 38°C. When the ambient temperature is 38°C, VO 2 It can play its heat insulation role, and this way is to reduce VO 2 Nanoparticle phase transitions in response to temperature, extending VO 2 An effective means to expand the application range of nanomaterials.
[0134] Example 10
[0135] In this example, the "sea urchin-shaped" W prepared in Example 5 18 O 49 and VO prepared in Example 1 2 Compounding was performed, and then a multilayer W was prepared according to the method of Example 9. 18 O 49 / VO 2 Intelligent waterproof and temperature-control film.
[0136] The multilayer W obtained in Example 10 18 O 49 / VO 2 Intelligent waterproof temperature control film and multilayer W obtained in Example 9 18 O 49 / VO 2The intelligent waterproof temperature control film was tested for thermal response temperature under the same conditions. The thermal response temperature test was: thermal insulation test under infrared irradiation for different time periods. The test results were: when infrared irradiation was 60s, VO 2 The thermal insulation temperature difference of the temperature control film is only 5.10℃. When the pure infrared irradiation lasts for 480s, the pure VO 2 The thermal insulation temperature difference of the temperature control film is 16.0℃, which is more obvious than that of a short-term infrared irradiation (60s). When the infrared irradiation is 60s, W 18 O 49 / VO 2 The thermal insulation temperature difference of the composite temperature control film is 14.7℃, and the temperature rises from 29.8℃ to 42.3℃. Under the condition of short-term infrared irradiation, its thermal insulation capacity is improved more greatly, which shows that the thermal response temperature is between 30℃ and 40℃. 18 O 49 Taking advantage of its excellent photothermal conversion efficiency, VO can be stimulated faster 2 Nanoparticles undergo phase transformation and play a heat-insulating role, which is to reduce VO 2 Nanoparticle phase transitions in response to temperature, extending VO 2 An effective means to expand the application range of nanomaterials.
[0137] In the present invention, W 18 O 49 Efficient photothermal conversion ability induces VO 2 Nanoparticles undergo reversible phase transition. On the other hand, W 18 O 49 High infrared shielding ability can also increase the thermal insulation performance of the film, synergistically optimizing VO 2 The film has intelligent temperature control performance. The obtained composite powder is modified and combined with FEVE resin to finally prepare VO with practical application value. 2 Thermochromic waterproof intelligent temperature control film is used for intelligent temperature control windows. More importantly, W 18 O 49 When oleic acid and oleylamine were used as surfactants, W 18 O 49 The morphology and size consistency of VO can be better controlled 2 The thermal response temperature is the most obvious improvement in the prior art.
[0138] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. High dispersion W 18 O 49 / VO 2 Nanocomposite powder, It is characterized in that It consists of granular VO 2 and lamellar W 18 O 49 The composite is prepared by mechanical stirring in a mixed solution of ethanol and polyethylene glycol according to a set mass ratio, wherein the lamellar W 18 O 49 The surface has oleic acid groups and oleylamine groups, which are used to make the lamellar W 18 O 49 The growth is hindered and the size is limited to a set range. The thickness of the layer is 5nm to 15nm, the length of the layer is 400nm ± 30nm, and the granular VO 2 The particle size is 40nm~80nm, granular VO 2 Evenly dispersed in the lamellar W 18 O 49 surface.
2. Preparation of the highly dispersible W as claimed in claim 1 18 O 49 / VO 2 Nanocomposite powder method, It is characterized in that The whole process adopts the hydrothermal method, which specifically includes the following steps: S1: Preparation of VO by hydrothermal method 2 Nano powder, S2: Preparation of W by hydrothermal method 18 O 19 Powder, specifically including the following sub-steps, S21: Add oleic acid and oleylamine to anhydrous ethanol, stir and mix evenly to obtain a mixed solvent, S22: Add tungsten chloride powder to the mixed solvent of step S21, and continue stirring until a golden yellow and transparent solution is obtained. S23: quickly transfer the golden yellow and transparent solution obtained in step S22 to a sealed container to prevent it from coming into contact with water vapor or being oxygenated, place the sealed container in a high-pressure reactor for hydrothermal reaction, and naturally cool to room temperature after the reaction to obtain a hydrothermal reaction product. S24: The hydrothermal product obtained in step S23 is centrifuged and washed, then vacuum dried, and finally ground to obtain W 18 O 49 Nano flake powder, Among them, step S1 and step S2 are in no particular order. S3: VO 2 Nanopowder and W 18 O 19 Nano-flaky powder is compounded.
3. The method according to claim 2, It is characterized in that In step S21, the volume ratio of anhydrous ethanol to the total volume of oleic acid and oleylamine is 80:3-80:5, and in step S22, the mass ratio of oleic acid to oleylamine to tungsten chloride powder is 9:2-9:
4.
4. The method according to claim 2, It is characterized in that In step S23, the temperature of the hydrothermal reaction is 160° C. to 190° C., and the time of the hydrothermal reaction is 22 h to 26 h.
5. The method according to any one of claims 2 to 4, It is characterized in that In step S1, VO is prepared 2 The specific steps of nano powder are: S11: Dissolve ammonium metavanadate in deionized water and stir evenly to obtain a milky white ammonium salt suspension. S12: Dissolve the reducing agent hydrazine monohydrochloride in water and stir until completely dissolved. Then add the milky white ammonium salt suspension dropwise. After the solution turns brown, continue stirring. Add concentrated hydrochloric acid dropwise. After the solution turns into a blue clear solution, continue stirring. S13: using ammonia water as a precipitant, adding the blue clear solution dropwise, and when the blue clear solution gradually changes to brownish yellow earth color, adjusting its pH, continuing to stir, obtaining a precipitate, and washing the precipitate by centrifugation. S14: The brown-yellow earth-colored precipitate washed by centrifugation is transferred to a container, ultrapure water is added to obtain a precursor, and the precursor is placed in a reactor for hydrothermal reaction to obtain a hydrothermal reaction product. S15: The hydrothermal reaction product is centrifuged and washed, vacuum dried and fully ground to obtain VO 2 Powder, VO 2 The powder particle size is 40 to 80 nm.
6. The method according to claim 5, It is characterized in that In step S13, the pH is adjusted to 8-8.
6. In step S14, the temperature of the hydrothermal reaction is 260-290° C., and the time of the hydrothermal reaction is 22-26 hours.
7. The method according to claim 6, It is characterized in that In step S3, VO 2 Nanopowder and W 18 O 19 The specific process of compounding nano-flaky powder is as follows: The VO obtained in step S1 is 2 Nanopowder and step S2 to obtain W 18 O 49 The nano-flaky powder is added to a mixed solution of ethanol and polyethylene glycol in a mass ratio of 4:1 to 1:1 and mechanically stirred. In the mixed solution of ethanol and polyethylene glycol, the mass ratio of ethanol and polyethylene glycol is 50:3 to 50:
5. After the stirring is completed, the product is washed and dried, and then ground to obtain W 18 O 49 / VO 2 Composite powder.
8. The highly dispersible W according to claim 1 18 O 49 / VO 2 Application of nanocomposite powders, It is characterized in that The invention is used for preparing thermochromic temperature-controlling film.
9. The highly dispersible W as claimed in claim 8 18 O 49 / VO 2 Application of nanocomposite powders, It is characterized in that Adopt polytrifluoroethylene / vinyl ether resin mixed with high dispersibility W 18 O 49 / VO 2 Nanocomposite powders for the preparation of thermochromic temperature-controlling films with high dispersion W 18 O 49 / VO 2 The mass ratio of the nano-composite powder to the polychlorotrifluoroethylene / vinyl ether resin is 0.1:5-0.2:5, and the obtained thermochromic temperature-controlling film has a thermal response temperature of 30°C-40°C.
Citation Information
Patent Citations
Composite dispersion film and preparation method thereof
CN115057625A