Preparation method of polyethylene sound-absorbing spillplate
By mixing the crosslinking agent-modified graphene, wear-resistant agent, processing aid and microbeads with polyethylene and crosslinking under irradiation conditions, the problem of insufficient performance of the polyethylene coal barrier is solved, and a high-strength is prepared , polyethylene sound-absorbing coal plate with wear resistance and antistatic properties is suitable for high-performance materials needs in the coal mining industry.
Patent Information
- Application Number
- CN202411222673.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
The existing polyethylene coal barrier plates have shortcomings in impact resistance, wear resistance and mechanical properties, and are difficult to meet the high-performance needs of the coal mine industry.
Graphene, wear-resistant agent, processing aid and microbeads modified with crosslinking agent were mixed with polyethylene and then injection molded, and crosslinked under irradiation conditions to prepare high strength, wear resistance and anti-static properties. polyethylene sound absorbing coal slab.
It significantly improves the mechanical properties, wear resistance and impact resistance of the coal barrier plate, extends its service life, and enhances the antistatic and sound absorption properties, which is suitable for the high-performance material needs of the coal mine industry.
Smart Images

Figure CN119081261A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyethylene coal-blocking plate materials, and in particular to a method for preparing a polyethylene sound-absorbing coal-blocking plate. Background Art
[0002] With the continuous progress and innovation of modern coal mining technology, coal mining operations are undergoing a transformation from traditional manual mining to modern mechanized operations, and even towards an automated future. There are abundant coal resources in the vast coal mines. However, iron sulfide nodules are often present in thin coal seam mining areas, and their extremely high hardness poses a huge challenge to coal mining. Traditional coal mining machine picks are difficult to cut iron sulfide nodules, so the blasting coal dropping process is widely used. In this process, the coal discharge process requires a lot of manpower and time. The current commonly used treatment method is to use a scraper conveyor to transport coal. The coal blocking plate installed on the pipe guard near the side chute of the scraper conveyor near the goaf plays a vital role. Its function is to block the blasting coal from rushing to the goaf, ensure that the coal is recovered into the scraper conveyor, avoid the waste of resources, and realize the automatic loading of coal.
[0003] At present, the performance requirements for coal retaining plates are increasing. Construction sites that use blasting coal dropping methods require coal retaining plates to be able to withstand the huge impact force from blasting activities and have excellent impact resistance to avoid deformation. At the same time, during the automated transportation process, the coal retaining plates need to withstand long-term friction and wear, reduce the frequency of replacement, and improve production efficiency and safety. Therefore, the coal retaining plates need to have multiple properties such as excellent bending resistance, wear resistance, impact resistance, hydrolysis resistance, acid and alkali corrosion resistance, and oil resistance to extend the service life of the coal retaining plates. At present, polymer polyethylene materials are the main materials used to manufacture coal retaining plates, but their wear resistance needs to be improved, their mechanical properties under hydrolysis conditions decrease rapidly, and their strength still has room for improvement. Therefore, it is necessary to effectively improve the polyethylene matrix to improve the long-term performance of the coal retaining plates. In short, the development of a polyethylene coal retaining plate with high strength, wear resistance, antistatic and sound absorption is crucial to the development of the coal mining industry. Summary of the invention
[0004] The main purpose of the present invention is to provide a method for preparing a polyethylene sound-absorbing coal-blocking plate, so as to solve the problem of poor performance of the polyethylene coal-blocking plate in the prior art.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a polyethylene sound-absorbing coal-blocking board is provided, the method comprising: mixing and molding graphene modified by a cross-linking agent, a wear-resistant agent, a processing aid, microbeads and polyethylene to obtain the above-mentioned polyethylene sound-absorbing coal-blocking board.
[0006] Furthermore, the preparation method of the above-mentioned cross-linker-modified graphene is as follows: mixing a graphene dispersion with a cross-linker to obtain a mixed solution to be cross-linked; and subjecting the above-mentioned mixed solution to be cross-linked to microwave irradiation functionalization treatment to obtain the above-mentioned cross-linker-modified graphene.
[0007] Furthermore, the preparation method of the above-mentioned graphene dispersion includes: mixing graphite powder, a dispersant and ultrapure water to obtain a graphite mixed suspension; and subjecting the above-mentioned graphite mixed suspension to liquid phase shear exfoliation to obtain the above-mentioned graphene dispersion.
[0008] Furthermore, the concentration of the cross-linking agent is 0.05-2 mol / L.
[0009] Furthermore, the crosslinking agent is selected from any one or more of the following: polyetherimide M w =10 4 ~10 5 Da, polyamino polyallylamine M w =10 3 ~10 4 Da, polydopamine M w =10 3 ~10 4 Da, polyurethane imine M w =10 3 ~10 5 Da, tris(hydroxymethyl)aminomethane, cross-linked polystyrene-divinylbenzenesulfonic acid or γ-aminopropyltriethoxysilane.
[0010] Furthermore, the molar ratio of the graphene dispersion to the cross-linking agent is 100:1 to 40:3.
[0011] Furthermore, the apparatus for carrying out the above microwave irradiation functionalization treatment is a microwave reactor, the reaction temperature is 90-100° C., and the reaction time is 5-25 min.
[0012] Furthermore, the water content of the cross-linker-modified graphene is 5% to 7%; preferably, the water content of the cross-linker-modified graphene after spray drying or vacuum freeze drying is 0.5% to 0.7%; more preferably, the spray drying temperature is 120 to 200°C, and the liquid inlet rate of the cross-linker-modified graphene is 1 to 20 mL / min; more preferably, the vacuum freeze drying temperature is -20 to -5°C, the time is 8 to 48 hours, and the air pressure is 80 to 200 Pa.
[0013] Furthermore, the graphite is selected from any one or more of the following: microcrystalline graphite, thermally expanded graphite or highly oriented pyrolytic graphite; preferably, the mass concentration of the graphite in the graphite mixed suspension is 0.5-1%.
[0014] Furthermore, the above-mentioned dispersant is selected from any one or more of the following: N-methylpyrrolidone, sodium dodecylbenzenesulfonate, sodium taurodeoxycholate, dimethylformamide, ethanol, o-dichlorobenzene or poloxamer; preferably, the mass ratio of the above-mentioned graphite to the above-mentioned dispersant is 80:1 to 100:1.
[0015] Furthermore, the instrument used for the above-mentioned liquid phase shear exfoliation is selected from any one or more of the following: a nano bead mill, a pin sand mill, a turbine sand mill or a 2000 bar high-pressure homogenizer; preferably, the stirring treatment time is 30 to 60 minutes, the grinding speed is 800 to 1000 r / min, and the grinding time is 1.2 to 5 hours; preferably, the above-mentioned graphene dispersion includes one or more layers of graphene layers, the average number of layers of the above-mentioned graphene layers is 10 to 20 layers, and the mass concentration of the above-mentioned graphene in the above-mentioned graphene dispersion is 2 to 8%.
[0016] Furthermore, the wear-resistant agent is selected from any one or more of the following: polytetrafluoroethylene M w =10 3 ~10 4 Da, ultra-high molecular weight polyurethane M w =10 4 ~10 5 Da, molybdenum disulfide, polysiloxane M w =10 3 ~10 4 Da, glass fiber, carbon fiber or aramid fiber.
[0017] Furthermore, the processing aid is selected from any one or more of the following: dibasic lead phosphite, methyl tin, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate or 2,6-di-tert-butyl-4-methylphenol.
[0018] Furthermore, the microbeads are organic microbeads or inorganic microbeads; the organic microbeads are selected from hybrid silicone microbeads; the inorganic microbeads are selected from any one or more of the following: 920DET40d25 microbeads, DU2201L microbeads or hollow glass microbeads.
[0019] Furthermore, the molecular weight of the polyethylene is 10,000 to 1,000,000.
[0020] Furthermore, the mass ratio of the cross-linking agent modified graphene to the wear-resistant agent is 12:1 to 2:1; the mass ratio of the wear-resistant agent to the polyethylene is 1:100 to 10:100; the mass ratio of the processing aid to the polyethylene is 1:1200 to 1:100; the mass ratio of the microbeads to the polyethylene is 1:100 to 12:100.
[0021] Furthermore, the mixed molding method includes: injection molding, mixed granulation followed by compression molding or extrusion blending molding; preferably, the instrument used for the injection molding is an injection molding machine, the injection pressure of the injection molding machine is 60-160 bar, the barrel temperature is 130-220° C., the melting temperature is 180-250° C., the mold temperature is 20-100° C., and the thickness of the injection molding sheet is 10-500 mm;
[0022] Preferably, the instrument used for the above-mentioned compression molding is a plate molding machine, the upper and lower mold temperatures of the above-mentioned plate molding machine are 160-190°C, the pressure is 1-10MPa, the time is 10-30min, and the thickness of the molded plate is 5-550mm; Preferably, the instrument used for the above-mentioned extrusion blending molding is a plate extruder, the screw speed of the above-mentioned plate extruder is 5-30r / min, the compression section temperature is 80-150°C, the homogenization section temperature is 150-200°C, the die temperature is 190-220°C, and the extruded plate thickness is 2-500mm.
[0023] Furthermore, after the molding is completed, the preparation method further comprises irradiating the polyethylene sound-absorbing coal-blocking board to obtain an irradiated polyethylene sound-absorbing coal-blocking board; preferably, the irradiation source for the irradiation is selected from any one or more of the following: a high-energy electron beam or a Co 60 Preferably, the irradiation dose is 20 to 110 kGy; the irradiation rate is 0.5 to 1.0 kGy / h; the crosslinking density after irradiation is 100 to 550 mol / m 3 .
[0024] By applying the technical solution of the present invention, a polyethylene sound-absorbing coal-blocking plate is obtained by mixing graphene modified by a cross-linking agent, a wear-resistant agent, a processing aid, microbeads and polyethylene, and then injection molding and cross-linking under irradiation conditions. The present invention solves the problem of poor mechanical properties of polyethylene sound-absorbing coal-blocking plates in the prior art. The coal-blocking plate prepared by the solution of the present invention has strong mechanical properties, strong wear resistance, antistatic and sound-absorbing properties, and shows broad prospects for application in the coal mining industry. It provides new ideas and methods for the design and manufacture of high-performance polyethylene sound-absorbing coal-blocking plate materials, and has far-reaching significance for the development of the coal mining industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 A schematic diagram of a method for preparing a polyethylene sound-absorbing coal baffle according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present invention can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0028] As mentioned in the background art, the coal baffles in the prior art have poor performance and high wear rate, which cannot meet the development needs of the coal mining industry. Therefore, in the present invention, the inventors tried to mix graphene modified by a cross-linking agent, a wear-resistant agent, a processing aid, microbeads and polyethylene, and then injection molded and cross-linked under irradiation conditions to obtain a polyethylene sound-absorbing coal baffle (see Figure 1 ), in order to improve the problem of poor performance of polyethylene coal retaining plates in the prior art, a series of protection schemes of the present invention are proposed.
[0029] In a first typical embodiment of the present invention, a method for preparing a polyethylene sound-absorbing coal-blocking board is provided, the method comprising: mixing and molding graphene modified with a cross-linking agent, a wear-resistant agent, a processing aid, microbeads and polyethylene to obtain the polyethylene sound-absorbing coal-blocking board.
[0030] There are various methods for preparing the crosslinker-modified graphene, and different preparation methods can be selected according to factors such as the selected crosslinker and the properties of the graphene. In a preferred embodiment of the present invention, the method for preparing the crosslinker-modified graphene is as follows: mixing a graphene dispersion with a crosslinker to obtain a mixed solution to be crosslinked; performing microwave irradiation functionalization treatment on the mixed solution to be crosslinked to obtain the crosslinker-modified graphene.
[0031] The microwave-assisted cross-linking method may help improve the mechanical properties of the material by providing functional sites and improving the compatibility of graphene and the cross-linking agent, while improving the antistatic properties by improving the conductive properties. The instrument for the microwave irradiation functionalization treatment is a microwave reactor, the reaction temperature is 90-100°C, and the reaction time is 5-25 minutes. Under these conditions, microwave-assisted cross-linking not only helps to reduce the relative sliding between graphene layers, but also may reduce the obstacles to electron transmission.
[0032] There are many types of cross-linking agents, and different technical solutions also have different selections of cross-linking agents. In a preferred embodiment of the present invention, the cross-linking agent is selected from any one or more of the following: polyetherimide M w =10 4 ~10 5 Da, polyamino polyallylamine M w =10 3 ~10 4 Da, polydopamine M w =10 3 ~10 4 Da, polyurethane imine M w =103 ~10 5 Da, tris(hydroxymethyl)aminomethane, cross-linked polystyrene-divinylbenzenesulfonic acid or γ-aminopropyltriethoxysilane. The molar ratio of the graphene dispersion to the cross-linking agent is 100:1 to 40:3. The concentration of the cross-linking agent is 0.05 to 2 mol / L. The application of the cross-linking agent can improve the compatibility between the wear-resistant agent and polyethylene during injection molding, thereby increasing the cross-linking density of the coal retaining plate and preventing mechanical relaxation.
[0033] The water content of the crosslinker-modified graphene is 5% to 7%; preferably, the water content of the crosslinker-modified graphene after drying is 0.5% to 0.7%; in a preferred embodiment of the present invention, the drying process is carried out by spray drying, preferably, the temperature of the spray drying is 120 to 200°C, and the liquid inlet rate of the crosslinker-modified graphene is 1 to 20 mL / min. Drying the crosslinker-modified graphene under these conditions has the beneficial effect of avoiding the destruction of the graphene material structure caused by excessive heating at a suitable temperature and liquid inlet rate.
[0034] In another preferred embodiment of the present invention, vacuum freeze drying is used for drying, and the vacuum freeze drying temperature is -20 to -5°C, the time is 8 to 48 hours, and the air pressure is 80 to 200 Pa. Using the above vacuum freeze drying technology to dry the crosslinker-modified graphene has the beneficial effects of maintaining the structural integrity and chemical stability of the graphene, avoiding thermal damage and oxidation, and improving the drying efficiency and uniformity of the material, and is suitable for large-scale production.
[0035] There are various methods for preparing the above-mentioned graphene dispersion. In a preferred embodiment of the present invention, the method for preparing the graphene dispersion includes: mixing graphite powder, a dispersant and ultrapure water to obtain a graphite mixed suspension; and subjecting the above-mentioned graphite mixed suspension to liquid phase shear exfoliation to obtain the above-mentioned graphene dispersion.
[0036] The graphite is selected from any one or more of the following: microcrystalline graphite, thermally expanded graphite or highly oriented pyrolytic graphite; preferably, the mass concentration of the graphite in the graphite mixed suspension is 0.5-1%. The use of the graphite to prepare the graphene dispersion has the beneficial effects of improving the stability and uniformity of the dispersion and enhancing the electrical conductivity and thermal conductivity of the graphene.
[0037] The dispersant is selected from any one or more of the following: N-methylpyrrolidone, sodium dodecylbenzenesulfonate, sodium taurodeoxycholate, dimethylformamide, ethanol, o-dichlorobenzene or poloxamer; preferably, the mass ratio of the graphite to the dispersant is 80:1 to 100:1. The dispersant helps to evenly disperse the graphene sheets in the dispersion when preparing the graphene dispersion, and increases the stability and dispersibility of the graphene dispersion.
[0038] Liquid phase shear exfoliation helps to improve the efficiency of obtaining graphene dispersion and helps to modify the surface of graphene. The instrument used for the above-mentioned liquid phase shear exfoliation is selected from any one or more of the following: nano bead mill, pin sand mill, turbine sand mill or 2000 bar high-pressure homogenizer; preferably, the stirring treatment time is 30 to 60 minutes, the grinding speed is 800 to 1000 r / min, and the grinding time is 1.2 to 5 hours; preferably, the above-mentioned graphene dispersion includes one or more layers of graphene layers, the average number of layers of the above-mentioned graphene layers is 10 to 20 layers, and the mass concentration of the above-mentioned graphene in the above-mentioned graphene dispersion is 2 to 8%.
[0039] The use of anti-wear agents to prepare coal-blocking plates has the beneficial effect of enhancing the wear resistance of the coal-blocking plates. In addition, the addition of anti-wear agents also enhances the fluidity of the melt during injection molding, thereby improving the molding efficiency of the coal-blocking plates. The anti-wear agents are selected from any one or more of the following: polytetrafluoroethylene M w =M w =10 3 ~10 4 Da, ultra-high molecular weight polyurethane M w =M w =10 4 ~10 5 Da, molybdenum disulfide, polysiloxane M w =M w =10 3 ~10 4 Da, glass fiber, carbon fiber or aramid fiber.
[0040] The function of the processing aid in the present invention is to improve the overall performance of the polyethylene sound-absorbing coal baffle, including anti-oxidation and thermal stability. The processing aid is selected from any one or more of the following: dibasic lead phosphite, methyl tin, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate or 2,6-di-tert-butyl-4-methylphenol.
[0041] Microwaves help to enhance the sound wave absorption capacity of the polyethylene coal baffle. The microbeads are organic microbeads or inorganic microbeads; the organic microbeads are selected from hybrid organic silicon microbeads; the inorganic microbeads are selected from any one or more of the following: 920DET40d25 microbeads, DU2201L microbeads or hollow glass microbeads.
[0042] The molecular weight of polyethylene has an important influence on the preparation of the coal retaining plate. The molecular weight of the above polyethylene is 10000-1000000. The above polyethylene is selected to prepare the coal retaining plate, which has excellent mechanical strength, processing performance, wear resistance and chemical stability, while optimizing the beneficial effect of cost-effectiveness.
[0043] The mass ratio of the cross-linking agent modified graphene to the wear-resistant agent is 12:1 to 2:1; the mass ratio of the wear-resistant agent to the polyethylene is 1:100 to 10:100; the mass ratio of the processing aid to the polyethylene is 1:1200 to 1:100; the mass ratio of the microbeads to the polyethylene is 1:100 to 12:100. The coal retaining plate prepared according to the above ratios has the beneficial effects of optimizing wear resistance, processing performance, impact resistance, chemical corrosion resistance and thermal stability, while balancing cost-effectiveness and comprehensive performance.
[0044] The mixed molding methods include: injection molding, mixed granulation followed by compression molding or extrusion blending molding. The polyethylene sound-absorbing coal-blocking board obtained by different molding methods has different characteristics, which can meet the different market requirements for the properties of polyethylene sound-absorbing coal-blocking board.
[0045] In a preferred embodiment of the present invention, the instrument used for the above-mentioned injection molding is an injection molding machine, the injection pressure of the above-mentioned injection molding machine is 60-160 bar, the barrel temperature is 130-220°C, the melting temperature is 180-250°C, the mold temperature is 20-100°C, and the thickness of the injection molding plate is 10-500 mm. The use of injection molding to manufacture coal baffles can meet the market demand for coal baffles of different shapes. In addition, injection molding adopts fully automated molding technology, which is efficient and low in cost, and can meet the needs of large-scale production of coal baffles.
[0046] In another preferred embodiment of the present invention, the instrument used for compression molding is a plate molding machine, the upper and lower mold temperatures of the plate molding machine are 160-190°C, the pressure is 1-10 MPa, the time is 10-30 min, and the thickness of the molded plate is 5-550 mm. Compression molding technology uses high pressure to make the materials more tightly combined, significantly improves the mechanical strength of the coal baffle, and effectively improves the impact resistance and pressure resistance of the coal baffle. In the manufacturing process of the coal baffle, compression molding technology can ensure the uniformity and stability of the material, thereby improving the durability and reliability of the coal baffle.
[0047] In the third preferred embodiment of the present invention, the instrument used for extrusion blending is a sheet extruder, the screw speed of the sheet extruder is 5-30r / min, the compression section temperature is 80-150°C, the homogenization section temperature is 150-200°C, the die temperature is 190-220°C, and the thickness of the extruded sheet is 2-500mm. Extrusion blending can ensure the uniform mixing of the polyethylene matrix and additives (such as graphene, anti-wear agents, etc.) in a molten state, thereby improving the overall performance of the coal retaining plate. Through blending, the formula can be adjusted to optimize its key properties such as wear resistance, impact resistance, and antistatic properties according to the specific application requirements of the coal retaining plate.
[0048] The purpose of irradiation is to increase the cross-linking density of the material, thereby improving the mechanical properties, wear resistance and impact resistance of the coal retaining plate. In a preferred embodiment of the present invention, after the molding is completed, the preparation method further includes irradiating the polyethylene sound-absorbing coal retaining plate to obtain an irradiated polyethylene sound-absorbing coal retaining plate; preferably, the irradiation source for the above irradiation is selected from any one or more of the following: high-energy electron beam or Co 60 Preferably, the irradiation dose is 20 to 110 kGy; the irradiation rate is 0.5 to 1.0 kGy / h; the crosslinking density after irradiation is 100 to 550 mol / m 3 .
[0049] Irradiation treatment under the above conditions enhances the compatibility of graphene and polyethylene, thereby significantly improving the crosslinking density of the polyethylene sound-absorbing coal-blocking board, including an increase in chemical crosslinking structures and physical entanglement structures, and enhancing the mechanical properties, wear resistance and impact resistance of the coal-blocking board. At the same time, the increase in crosslinking density caused by irradiation further enhances the antistatic properties and noise reduction effect of the polyethylene sound-absorbing coal-blocking board. Improving the performance of polyethylene sound-absorbing coal-blocking boards helps to extend the service life of coal-blocking boards, which is of great significance to the development of the coal mining industry.
[0050] By precisely controlling the irradiation conditions, the present invention not only achieves precise regulation of material properties, but also avoids plastic deformation of the material under high-intensity use conditions, thereby significantly improving the reuse rate of the coal retaining plate.
[0051] The beneficial effects of the present invention will be further explained in detail below in conjunction with specific embodiments.
[0052] Example 1
[0053] S11. Preparation of graphene dispersion: Place graphite (microcrystalline graphite, 5 g) and dispersant (N-methylpyrrolidone / sodium dodecylbenzenesulfonate = 2:1) in 1 L of ultrapure water and stir evenly. The mass ratio of graphite to dispersant is 100:1. Liquid phase shear exfoliation technology (nano bead mill, stirring time of 30 min, grinding speed of 800 r / min, grinding time of 5 h) is used to prepare graphene dispersion. The average number of graphene layers obtained is 10, and the mass / volume concentration of graphene is 2%.
[0054] S12. Preparation of crosslinker-modified graphene: The crosslinker (polyetherimide / polyaminopolyallylamine=1:3) was dissolved in ultrapure water, the volume ratio of graphene suspension to crosslinker solution (0.05 mol / L) was 100:1, and the crosslinker was loaded in a microwave reactor (reaction temperature was 100°C, reaction time was 5 min), and after the reaction was completed, the excess reactants were removed by spray drying (inlet temperature was 120°C, liquid inlet speed was 20 mL / min), and the crosslinker-modified graphene powder was obtained. The water content of the crosslinker-modified graphene before drying was 5%, and the water content of the crosslinker-modified graphene after drying was 0.5%.
[0055] S13. Preparation of high-performance coal-blocking plate: wear-resistant agent (polytetrafluoroethylene / ultra-high molecular weight polyethylene=1:5), processing aid (dibasic lead phosphite / methyl tin=2:1), organic / inorganic microbeads (920DET40d25 microbeads), cross-linking agent-modified graphene, and polyethylene pellets (molecular weight of 100,000) are mixed evenly (the mass ratio of cross-linking agent-modified graphene to wear-resistant agent is 12:1, the mass ratio of wear-resistant agent to polyethylene is 1:100, the mass ratio of processing aid to polyethylene is 1:1200, and the mass ratio of organic / inorganic microbeads to polyethylene is 1:100), and molded by injection molding machine (injection pressure of 60 bar, barrel temperature of 220°C, melting temperature of 180°C, and mold temperature of 20°C), and the plate thickness is 10 mm.
[0056] Example 2
[0057] S21. Preparation of graphene dispersion: Place graphite (thermal expansion graphite, 10 g) and dispersant (sodium taurodeoxycholate) in 1 L of ultrapure water and stir evenly. The mass ratio of graphite to dispersant is 80:1. Liquid phase shear exfoliation technology (nano-bead mill, stirring time of 60 min, grinding speed of 1000 r / min, grinding time of 1.2 h) is used to prepare graphene dispersion. The average number of graphene layers obtained is 20, and the mass / volume concentration of graphene is 8%.
[0058] S22. Preparation of crosslinker-modified graphene: crosslinker (polydopamine / polyethyleneimine = 1:4) was dissolved in ultrapure water, the volume ratio of graphene suspension to crosslinker solution (2 mol / L) was 40:3, placed in a microwave reactor to load the crosslinker (reaction temperature was 90°C, reaction time was 25 min), and after the reaction was completed, the excess reactants were removed by spray drying (inlet temperature was 200°C, liquid inlet speed was 1 mL / min) to obtain crosslinker-modified graphene powder. The water content of the crosslinker-modified graphene before drying was 7%, and the water content of the crosslinker-modified graphene after drying was 0.7%.
[0059] S23. Preparation of high-performance coal-blocking plate: the wear-resistant agent (ultra-high molecular weight polyethylene / molybdenum disulfide = 10:3), processing aid (dibasic lead phosphite / tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester = 5:1), organic / inorganic microbeads (hybrid silicone microbeads), cross-linking agent-modified graphene, and polyethylene pellets (molecular weight of 10,000) are mixed evenly (the mass ratio of cross-linking agent-modified graphene to wear-resistant agent is 2:1, the mass ratio of wear-resistant agent to polyethylene is 10:100, the mass ratio of processing aid to polyethylene is 12:1200, and the mass ratio of organic / inorganic microbeads to polyethylene is 12:100), and the plate is formed by an injection molding machine (injection pressure of 160 bar, barrel temperature of 130°C, melting temperature of 250°C, and mold temperature of 100°C), and the plate thickness is 500 mm.
[0060] Example 3
[0061] S31. Preparation of graphene dispersion: Place graphite (highly oriented pyrolytic graphite, 8 g) and dispersant (dimethylformamide / ethanol = 5:1) in 1 L of ultrapure water and stir evenly. The mass ratio of graphite to dispersant is 90:1. Use liquid phase shear exfoliation technology (turbine sand mill, stirring time of 40 min, grinding speed of 900 r / min, grinding time of 3 h) to prepare graphene dispersion. The average number of graphene layers obtained is 12, and the mass / volume concentration of graphene is 3%.
[0062] S32. Preparation of crosslinker-modified graphene: crosslinker (polyetherimide / polyaminopolyallylamine=1:3) was dissolved in ultrapure water, the volume ratio of graphene suspension to crosslinker solution (1 mol / L) was 40:1, placed in a microwave reactor to load the crosslinker (reaction temperature was 95°C, reaction time was 15 min), and after the reaction was completed, spray drying (inlet temperature was 140°C, liquid inlet speed was 18 mL / min) was used to remove excess reactants to obtain crosslinker-modified graphene powder. The water content of the crosslinker-modified graphene before drying was 6%, and the water content of the crosslinker-modified graphene after drying was 0.6%.
[0063] S33. Preparation of high-performance coal-blocking plate: the wear-resistant agent (polydopamine / trishydroxymethylaminomethane = 10:1), processing aid (tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester / 2,6-di-tert-butyl-4-methylphenol = 1:1), organic / inorganic microbeads (DU2201L microbeads), cross-linking agent-modified graphene, and polyethylene pellets (molecular weight of 15,000) are mixed evenly (the mass ratio of cross-linking agent-modified graphene to wear-resistant agent is 8:1, the mass ratio of wear-resistant agent to polyethylene is 3:100, the mass ratio of processing aid to polyethylene is 2:1200, and the mass ratio of organic / inorganic microbeads to polyethylene is 3:100), and the plate is molded by an injection molding machine (injection pressure of 80 bar, barrel temperature of 140°C, melting temperature of 210°C, and mold temperature of 40°C), and the plate thickness is 100 mm.
[0064] Example 4
[0065] S41. Preparation of graphene dispersion: Place graphite (thermal expansion graphite, 20 g) and dispersant (ethanol / o-dichlorobenzene / poloxamer = 5:2:2) in 1 L of ultrapure water and stir evenly. The mass ratio of graphite to dispersant is 100:3. Liquid phase shear exfoliation technology (nano-bead mill, stirring time of 20 min, grinding speed of 2000 r / min, grinding time of 1 h) is used to prepare graphene dispersion. The average number of graphene layers obtained is 8, and the mass / volume concentration of graphene is 15%.
[0066] S42. Preparation of crosslinker-modified graphene: crosslinker (crosslinked polystyrene-divinylbenzenesulfonic acid / γ-aminopropyltriethoxysilane=1:1) was dissolved in ultrapure water, the volume ratio of graphene suspension to crosslinker solution (2.5 mol / L) was 10:1, placed in a microwave reactor to load the crosslinker (reaction temperature was 160°C, reaction time was 35 min), and after the reaction was completed, spray drying (inlet temperature was 210°C, liquid inlet speed was 22 mL / min) was used to remove excess reactants to obtain crosslinker-modified graphene powder. The water content of crosslinker-modified graphene before drying was 4%, and the water content of crosslinker-modified graphene after drying was 0.4%.
[0067] S43. Preparation of high-performance coal-blocking plate: wear-resistant agent (ultra-high molecular weight polyethylene / glass fiber = 10:1), processing aid (dibasic lead phosphite / 2,6-di-tert-butyl-4-methylphenol = 5:1), organic / inorganic microbeads (hollow glass microbeads), cross-linking agent-modified graphene, and polyethylene pellets (molecular weight of 120,000) are mixed evenly (the mass ratio of cross-linking agent-modified graphene to wear-resistant agent is 1:1, the mass ratio of wear-resistant agent to polyethylene is 12:100, the mass ratio of processing aid to polyethylene is 13:1200, and the mass ratio of organic / inorganic microbeads to polyethylene is 15:100), and the plate thickness is 4 mm in an injection molding machine (injection pressure is 180 bar, barrel temperature is 120°C, melting temperature is 260°C, and mold temperature is 120°C).
[0068] Example 5
[0069] The difference from Example 1 is:
[0070] 1) The molding method is to place the sheet in a sheet extruder (the screw type is an equal-depth unequal-pitch gradient type, the screw speed is 30 r / min, the compression section temperature is 80°C, the homogenization section temperature is 200°C, and the die temperature is 220°C), and the sheet thickness is 500 mm.
[0071] 2) After forming, further irradiation treatment is carried out, and the irradiation conditions are: using a radiation source Co 60 The plate was irradiated with an irradiation dose of 20 kGy and an irradiation rate of 1.0 kGy / h. The crosslinking density after irradiation was 100 mol / m 3 .
[0072] 3) After the microwave reaction, the excess reactants were removed by vacuum freeze drying (the temperature of the freezing chamber was -20°C, the air pressure in the freezing chamber was 200 Pa, and the drying time was 8 hours) to obtain the cross-linker-modified graphene powder. The water content of the cross-linker-modified graphene before drying was 5%. The water content of the cross-linker-modified graphene after drying was 0.7%.
[0073] The rest is the same as in Example 1.
[0074] Example 6
[0075] The difference from Example 2 is:
[0076] 1) The molding method is to place the sheet in a sheet extruder (the screw type is an equidistant and unequal depth gradient type, the screw speed is 5r / min, the compression section temperature is 150°C, the homogenization section temperature is 150°C, and the die temperature is 190°C), and the sheet thickness is 2mm.
[0077] 2) After forming, further irradiation treatment is carried out. The irradiation conditions are: the plate is irradiated with a high-energy electron beam, the irradiation dose is 110 kGy, the irradiation rate is 0.5 kGy / h, and the crosslinking density after irradiation is 550 mol / m 3 .
[0078] 3) After the microwave reaction, the excess reactants were removed by freeze drying (the temperature of the freezing chamber was -5°C, the air pressure in the freezing chamber was 80 Pa, and the drying time was 48 hours) to obtain cross-linker-modified graphene powder. The water content of the cross-linker-modified graphene before drying was 6%. The water content of the cross-linker-modified graphene after drying was 0.6%.
[0079] The rest is the same as Example 2.
[0080] Example 7
[0081] The difference from Example 3 is:
[0082] 1) The molding method is to place it in a sheet extruder (the screw type is a sudden type, the screw speed is 10r / min, the compression section temperature is 95°C, the homogenization section temperature is 160°C, and the die temperature is 200°C), and the sheet thickness is 10mm.
[0083] 2) After forming, further irradiation treatment is carried out. The irradiation conditions are: the plate is irradiated with a high-energy electron beam, the irradiation dose is 40 kGy, the irradiation rate is 0.6 kGy / h, and the crosslinking density after irradiation is 240 mol / m 3 .
[0084] 3) After the reaction is completed, freeze drying (the temperature of the freezing chamber is -15°C, the air pressure in the freezing chamber is 150Pa, and the drying time is 24 hours) is used to remove excess reactants to obtain crosslinker-modified graphene powder. The water content of the crosslinker-modified graphene before drying is 7%. The water content of the crosslinker-modified graphene after drying is 0.5%.
[0085] The rest is the same as in Example 3.
[0086] Example 8
[0087] The difference from Example 4 is:
[0088] 1) The molding method is to place it in a plate extruder (the screw type is a sudden type, the screw speed is 40r / min, the compression section temperature is 160°C, the homogenization section temperature is 220°C, and the die temperature is 230°C), and the plate thickness is 510mm.
[0089] 2) After the reaction is completed, the excess reactants are removed by vacuum freeze drying (the temperature of the freezing chamber is -30°C, the air pressure in the freezing chamber is 210Pa, and the drying time is 50 hours) to obtain crosslinker-modified graphene powder. The water content of the crosslinker-modified graphene before drying is 4%. The water content of the crosslinker-modified graphene after drying is 0.2%.
[0090] The rest is the same as Example 4.
[0091] Example 9
[0092] The difference from Example 1 is:
[0093] The molding method is to mix and granulate and then place it in a plate molding machine (upper and lower mold temperatures are 160° C., pressure is 1 MPa, time is 10 min), and the plate thickness is 550 mm.
[0094] The rest is the same as in Example 1.
[0095] Example 10
[0096] The difference from Example 2 is:
[0097] The molding method is to mix and granulate and then place it in a plate molding machine (upper and lower mold temperatures are 190° C., pressure is 10 MPa, time is 30 minutes), and the plate thickness is 5 mm.
[0098] The rest is the same as Example 2.
[0099] Embodiment 11
[0100] The difference from Example 3 is:
[0101] The molding method is to place the mixed granules in a plate molding machine (upper and lower mold temperatures are 175° C., pressure is 4 MPa, and time is 12 min), and the plate thickness is 10 mm.
[0102] The rest is the same as in Example 3.
[0103] Example 12
[0104] The difference from Example 4 is:
[0105] The molding method is to place the mixed granules in a plate molding machine (upper and lower mold temperatures are 200° C., pressure is 12 MPa, and time is 32 minutes), and the plate thickness is 4 mm.
[0106] The rest is the same as Example 4.
[0107] Example 13 (Preparation of graphene dispersion without using a dispersant)
[0108] The difference from Example 1 is that no dispersant is used to prepare the graphene dispersion, but the graphite is directly subjected to liquid phase shear exfoliation in ultrapure water. The rest is the same as Example 1.
[0109] Example 14 (obtaining cross-linker-modified graphene without microwave-assisted method)
[0110] The difference from Example 2 is that the microwave-assisted method is not used to load the cross-linking agent to obtain the cross-linking agent-modified graphene. The rest is the same as Example 2.
[0111] Comparative Example 1 (without adding anti-wear agent)
[0112] The difference from Example 1 is that no anti-wear agent is added. The rest is the same as Example 1.
[0113] Comparative Example 2 (without adding processing aid)
[0114] The difference from Example 2 is that no processing aid is added. The rest is the same as Example 2.
[0115] Comparative Example 3 (without adding microbeads)
[0116] The difference from Example 3 is that no micro beads are added. The rest is the same as Example 3.
[0117] Comparative Example 4 (using graphene not modified by cross-linking agent)
[0118] The difference from Example 4 is that graphene not modified by a cross-linking agent is used. The rest is the same as Example 4.
[0119] Structural characterization and performance testing
[0120] Tensile performance test: The obtained polyethylene sound-absorbing coal-blocking board was cut to obtain tensile specimens, and the tensile performance of the board was tested using a universal tensile machine (model 4403, sensor 100N) of Instron Company of the United States according to the ASTM D638-2003 plastic tensile performance test standard of the American Society for Testing and Materials. At least 3 parallel test samples were guaranteed for each group, and the results were averaged.
[0121] Impact resistance test: The obtained polyethylene sound-absorbing coal-blocking board was cut to obtain standard specimens, and the impact resistance of the board was tested using a simple beam impact tester (model 9050) of the British Instron Instrument Group according to the plastic impact resistance test standard ASTM D4812-19 of the American Society for Testing and Materials. At least 3 parallel test specimens were guaranteed for each group, and the average value of the results was taken.
[0122] Tribological performance test: The wear resistance test of the sample is based on the standard of ASTM G132-96, and the test instrument is HSR-2M high-speed reciprocating friction and wear testing machine. GCR15 bearing steel balls with a diameter of 5mm are selected as the corresponding material. The steel ball loading load is 20N, the reciprocating frequency is 16.67Hz, the reciprocating length is 5mm, the friction time is 1000min, and the tribological properties are studied at room temperature after 1×106 reciprocating friction cycles. The wear amount (M, mg) is measured using a high-precision electronic balance, and the friction coefficient (ε) is calculated using the following formula (1):
[0123]
[0124] Where M1 (mg) is the wear amount of the standard sample, and M2 (mg) is the wear amount of the tested sample.
[0125] The instrument's electronic probe measures the wear volume (V, mm3) and calculates the wear rate (K, mm3 Nm-1) using the following formula (2):
[0126]
[0127] Where F(N) is the load during the friction test, and x(m) is the total sliding distance of 30 min. To ensure the accuracy of the experimental data, each sample was tested three times.
[0128] Antistatic performance test: Use 4339A / B type high insulation resistance tester to test the volume resistivity of each sample, clamp both ends of the sample with copper clips and test according to GB / T1410-2006.
[0129] Sound absorption performance test: A two-channel acoustic impedance tube is used to test the sound absorption coefficient of the sample. The sample thickness is 5mm and the diameter is 30mm. The sound wave frequency range is 100~5000Hz. The test is carried out in accordance with GB / T 18696.1-2004.
[0130] Vibration fatigue test: The exciter is used to apply an excitation signal to excite the polyethylene sound-absorbing coal baffle sample, and the POLYTEC laser vibration measurement system is used to scan and pick up the vibration response of each node of the sample. By controlling the excitation frequency of the vibration table to 30Hz, the specimen is in a resonant state. The strain gauge attached to the specimen is connected to the digital acquisition system, and the corresponding stress value is measured to obtain the maximum fatigue life and the fatigue limit stress at this time.
[0131] The properties of the polyethylene sound-absorbing coal-blocking plates prepared using the above-mentioned embodiments and comparative examples are shown in Table 1.
[0132] Table 1:
[0133]
[0134] The polyethylene sound-absorbing coal-blocking plates prepared in Examples 1 to 14 exhibited extremely high tensile strength (68.6 to 93.6 MPa) and impact strength (162.4 to 208.3 MPa), extremely high mechanical strength, and also had low friction coefficients (0.09 to 0.22) and wear rates (3.2×10 -5 ~8.7×10 -5 mm 3 N m -1 ), significantly improving the resistance of the polyethylene sound-absorbing coal-blocking board to friction erosion under cyclic friction. It is also of great significance that the polyethylene sound-absorbing coal-blocking boards of Examples 1 to 14 all have a relatively low volume resistivity (8.62×10 6 ~9.48×10 7 Ω·cm), showing excellent antistatic ability, which is very suitable for the antistatic needs of the coal retaining plate under high cycle friction during coal transportation, and has a high sound absorption coefficient (0.35-0.63), showing good sound absorption and noise reduction performance, and has unique advantages in dealing with the high noise environment where the coal retaining plate is used. In addition, the vibration fatigue cycle life (10.3×10 6 ~23.2×10 6 times) and ultimate stress (44.8~79.6MPa), which makes the coal retaining plate have more excellent actual service capacity.
[0135] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: the polyethylene sound-absorbing coal baffle prepared by the present invention not only achieves precise control of material properties, but also avoids plastic deformation of the material under high-intensity use conditions, significantly improving the reuse rate of the coal baffle. The improvement of these comprehensive properties makes the application of the polyethylene sound-absorbing coal baffle of the present invention on the scraper conveyor show a broad industrial application prospect, and provides new ideas and methods for the design and manufacture of high-performance polyethylene sound-absorbing coal baffle materials, which is of great significance to the development of the coal mining industry.
[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a polyethylene sound-absorbing coal-blocking plate, characterized in that: The preparation method comprises: The polyethylene sound-absorbing coal-blocking board is obtained by mixing and molding graphene modified by a cross-linking agent, a wear-resistant agent, a processing aid, microbeads and polyethylene.
2. The preparation method according to claim 1, characterized in that: The preparation method of the cross-linking agent modified graphene is as follows: Mixing the graphene dispersion with the cross-linking agent to obtain a mixed solution to be cross-linked; The mixed solution to be cross-linked is subjected to microwave irradiation functionalization treatment to obtain the cross-linking agent-modified graphene.
3. The preparation method according to claim 2, characterized in that: The preparation method of the graphene dispersion comprises: Mixing graphite powder, dispersant and ultrapure water to obtain a graphite mixed suspension; The graphite mixed suspension is subjected to liquid phase shear exfoliation to obtain the graphene dispersion.
4. The preparation method according to claim 2 or 3, characterized in that: The concentration of the cross-linking agent is 0.05-2 mol / L.
5. The preparation method according to claim 4, characterized in that: The crosslinking agent is selected from any one or more of the following: polyetherimide M w =10 4 ~10 5 Da, polyamino polyallylamine M w =10 3 ~10 4 Da, polydopamine M w =10 3 ~10 4 Da, polyurethane imine M w =10 3 ~10 5 Da, tris(hydroxymethyl)aminomethane, cross-linked polystyrene-divinylbenzenesulfonic acid or γ-aminopropyltriethoxysilane.
6. The preparation method according to claim 5, characterized in that: The molar ratio of the graphene dispersion to the cross-linking agent is 100:1 to 40:
3.
7. The preparation method according to claim 2, characterized in that: The instrument for carrying out the microwave irradiation functionalization treatment is a microwave reactor, the reaction temperature is 90-100° C., and the reaction time is 5-25 min.
8. The preparation method according to claim 2, characterized in that: The water content of the cross-linking agent modified graphene is 5% to 7%; Preferably, the water content of the cross-linking agent modified graphene after spray drying or vacuum freeze drying is 0.5% to 0.7%; More preferably, the spray drying temperature is 120-200° C., and the liquid feeding rate of the cross-linking agent-modified graphene is 1-20 mL / min; More preferably, the vacuum freeze-drying temperature is -20 to -5°C, the time is 8 to 48 hours, and the air pressure is 80 to 200 Pa.
9. The preparation method according to claim 3, characterized in that: The graphite is selected from any one or more of the following: microcrystalline graphite, thermally expanded graphite or highly oriented pyrolytic graphite; Preferably, the mass concentration of the graphite in the graphite mixed suspension is 0.5-1%.
10. The preparation method according to claim 3, characterized in that: The dispersant is selected from any one or more of the following: N-methylpyrrolidone, sodium dodecylbenzene sulfonate, sodium taurodeoxycholate, dimethylformamide, ethanol, o-dichlorobenzene or poloxamer; Preferably, the mass ratio of the graphite to the dispersant is 80:1 to 100:
1.
11. The preparation method according to claim 3, characterized in that: The instrument used for the liquid phase shear stripping is selected from any one or more of the following: a nano-bead mill, a pin-type sand mill, a turbine sand mill or a 2000 bar high-pressure homogenizer; Preferably, the stirring treatment time is 30 to 60 minutes, the grinding speed is 800 to 1000 r / min, and the grinding time is 1.2 to 5 hours; Preferably, the graphene dispersion comprises one or more graphene layers, the average number of graphene layers is 10 to 20, and the mass concentration of the graphene in the graphene dispersion is 2 to 8%.
12. The preparation method according to claim 1, characterized in that: The wear-resistant agent is selected from any one or more of the following: polytetrafluoroethylene M w =10 3 ~10 4 Da, ultra-high molecular weight polyurethane M w =10 4 ~10 5 Da, molybdenum disulfide, polysiloxane M w =10 3 ~10 4 Da, glass fiber, carbon fiber or aramid fiber.
13. The preparation method according to claim 1, characterized in that: The processing aid is selected from any one or more of the following: dibasic lead phosphite, methyl tin, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate or 2,6-di-tert-butyl-4-methylphenol.
14. The preparation method according to claim 1, characterized in that: The microbeads are organic microbeads or inorganic microbeads; the organic microbeads are selected from hybrid silicone microbeads; the inorganic microbeads are selected from any one or more of the following: 920DET40d25 microbeads, DU2201L microbeads or hollow glass microbeads.
15. The preparation method according to claim 1, characterized in that: The molecular weight of the polyethylene is 10,000 to 1,000,000.
16. The preparation method according to claim 1, characterized in that: The mass ratio of the cross-linking agent modified graphene to the wear-resistant agent is 12:1 to 2:1; the mass ratio of the wear-resistant agent to the polyethylene is 1:100 to 10:100; the mass ratio of the processing aid to the polyethylene is 1:1200 to 1:100; the mass ratio of the microbeads to the polyethylene is 1:100 to 12:
100.
17. The preparation method according to claim 1, characterized in that: The mixed molding method includes: injection molding, mixed granulation followed by compression molding or extrusion blending molding; Preferably, the instrument used for the injection molding is an injection molding machine, the injection pressure of the injection molding machine is 60-160 bar, the barrel temperature is 130-220° C., the melting temperature is 180-250° C., the mold temperature is 20-100° C., and the thickness of the injection molding plate is 10-500 mm; Preferably, the instrument used for the compression molding is a plate compression machine, the upper and lower mold temperatures of the plate compression machine are 160-190°C, the pressure is 1-10 MPa, the time is 10-30 min, and the thickness of the compression plate is 5-550 mm; Preferably, the instrument used for the extrusion blending molding is a sheet extruder, the screw speed of the sheet extruder is 5-30r / min, the compression section temperature is 80-150°C, the homogenization section temperature is 150-200°C, the die temperature is 190-220°C, and the extruded sheet thickness is 2-500mm.
18. The preparation method according to claim 1, characterized in that: After the molding is completed, the preparation method further comprises irradiating the polyethylene sound-absorbing coal-blocking board to obtain an irradiated polyethylene sound-absorbing coal-blocking board; Preferably, the radiation source for the irradiation is selected from any one or more of the following: high energy electron beam or Co 60 ; Preferably, the irradiation dose is 20 to 110 kGy; the irradiation rate is 0.5 to 1.0 kGy / h; and the crosslinking density after irradiation is 100 to 550 mol / m 3 .