Anti-aging insulated cable material and preparation method thereof

By introducing anti-aging reinforcement agents prepared by reactions such as 2-nitro m-diphenol in polyvinyl chloride, combined with aluminum nitride, the problem of degradation of polyvinyl chloride in ultraviolet light irradiation is solved, and its aging resistance is significantly improved and mechanical strength.

CN119081316AInactive Publication Date: 2024-12-06ANHUI XINYA STAR CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411490693.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyvinyl chloride is prone to degradation under outdoor ultraviolet light, resulting in a decline in mechanical properties. The existing ultraviolet absorbers will migrate and exudate for a long time, affecting their aging resistance.

Method used

The anti-aging enhancer prepared by reactions such as 2-nitrom-diphenol, oleic acid and sodium sulfide are used to form an anti-aging agent with a silane coupling agent structure through esterification, reduction and coupling reactions, and combined with aluminum nitride By adsorbing HCl and forming a mesh structure, the aging resistance of polyvinyl chloride is enhanced.

Benefits of technology

It significantly improves the aging resistance of polyvinyl chloride materials, inhibits the degradation of ultraviolet light energy on the material, extends the service life, and improves the mechanical strength and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to an anti-aging insulated cable material and a preparation method thereof, and belongs to the technical field of high polymer material modification, and the anti-aging insulated cable material comprises the following components in parts by weight: 100 parts of polyvinyl chloride resin, 15-20 parts of an anti-aging enhancer, 20-30 parts of a plasticizer, 25-30 parts of a flame retardant, 3-5 parts of aluminum nitride, 2-3 parts of an antioxidant, 2-3 parts of a light stabilizer, 2-3 parts of a heat stabilizer and 1-1.5 parts of a lubricant; the anti-aging enhancer is coupled with aluminum nitride to inhibit the light degradation effect of ultraviolet light energy on a polyvinyl chloride matrix, butoxy groups adsorb HCl generated due to light degradation, and unsaturated double structural bonds and a diene structure are subjected to addition, so that on one hand, product discoloration can be inhibited, and on the other hand, a net structure can be formed; the long alkyl chain and the polyvinyl chloride matrix molecular chain are mutually entangled to form an interpenetrating network, so that the migration ability of the anti-aging enhancer under the action of ultraviolet light energy is effectively inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material modification, and in particular relates to an aging-resistant insulating cable material and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC for short) is a general-purpose material with low price, corrosion resistance and low energy consumption. It is the second largest plastic variety in the world after polyethylene. It has good electrical insulation, flame retardancy, solvent resistance and good wear resistance, which makes it widely used in the production of cable materials and occupies an important position in insulating cable materials.

[0003] Cable materials are mostly used in outdoor environments. The molecular structure of PVC polymer will degrade and undergo chain dehydrochlorination under the action of outdoor ultraviolet light energy, and will form a dense conjugated diene structure. The HCI produced by degradation will catalyze the degradation of the polyvinyl chloride molecular chain by light energy, and the multi-olefin structure and structural defects will undergo oxidative decomposition reactions, thereby reducing the mechanical properties of the PVC material, and in the presence of oxygen, it will accelerate its chain dehydrochlorination. PVC is prone to discoloration and brittleness, resulting in deterioration of its performance.

[0004] In the prior art, ultraviolet absorbers are usually added to absorb the energy of ultraviolet light, thereby inhibiting the influence of ultraviolet light on the molecular chain of polyvinyl chloride polymers, reducing the generation of chain de-HCl and conjugated diene structures, and thus achieving the purpose of extending the service life of polyvinyl chloride polymers. However, ultraviolet absorbers are pure organic small molecule compounds. When directly added to the polyvinyl chloride, under the influence of ultraviolet light for a long time, the small molecule ultraviolet absorbers will migrate and seep out, resulting in a decrease in its ability to absorb ultraviolet light, thereby causing the mechanical strength of the polyvinyl chloride body to decrease under long-term ultraviolet light irradiation, further affecting the aging resistance of the polyvinyl chloride body, thereby limiting the application of polyvinyl chloride in the field of cable materials. Summary of the invention

[0005] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide an aging-resistant insulating cable material and a preparation method thereof; The purpose of the present invention can be achieved through the following technical solutions: An aging-resistant insulating cable material comprises the following raw materials in parts by weight: 100 parts of polyvinyl chloride resin, 15-20 parts of anti-aging enhancer, 20-30 parts of plasticizer, 25-30 parts of flame retardant, 3-5 parts of aluminum nitride, 2-3 parts of antioxidant, 2-3 parts of light stabilizer, 2-3 parts of heat stabilizer and 1-1.5 parts of lubricant; Preparation of anti-aging enhancer: Step A1: 2-nitro-m-diphenol, oleic acid, sodium hydroxide and DMF are mixed and added into a reaction kettle, the stirring reaction rate is controlled to be 200-300 r / min, the temperature is raised to 60-70° C., and the mixture is stirred for reaction for 3-4 hours, and then washed with water 3 times and dried to obtain an unsaturated ester intermediate; Further, the usage ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF is 1 mol: 2 mol: 2-3 g: 500 mL; In the above reaction, 2-nitro-meta-diphenol and oleic acid undergo an esterification reaction, and oleic acid is directly added to the 2-nitro-meta-diphenol molecule to introduce an unsaturated long-chain structure; the specific reaction process is as follows:

[0006] Step A2: taking an unsaturated ester intermediate, sodium sulfide and ethanol, mixing and feeding them into a reactor, controlling the stirring reaction rate to be 300-400 r / min, heating to 50-60° C., stirring and reacting for 1-2 hours, then adding 2,5-dihydroxyterephthalic acid and DCC, heating to 60-70° C., stirring and reacting for 3-5 hours, and then vacuum rotary evaporation to obtain an unsaturated amide-ester intermediate; Further, the usage ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2 mol: 30-40 g: 1 mol: 4-6 g: 1000 mL; In the above reaction, the unsaturated ester intermediate is reduced to an amino group under the reduction of sodium sulfide and reacts with 2,5-dihydroxyterephthalic acid to form a macromolecular organic substance. The structural formula of the unsaturated amide-ester intermediate is shown as follows:

[0007] Step A3: taking an unsaturated amide-ester intermediate, butyl bromide, anhydrous potassium carbonate and DMF, mixing and feeding them into a reactor, controlling the stirring reaction rate to be 350-450 r / min, heating to 80-90° C., stirring and reacting for 2-4 hours, then adding 3-chloropropyltrimethoxysilane and triethylamine, continuing the reaction for 1-2 hours, then extracting with ethyl acetate for 3 times, then extracting the ethyl acetate phase with water, and finally evaporating in vacuo to obtain an anti-aging enhancer; Further, the usage ratio of the unsaturated amide-ester intermediate, butyl bromide, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1 mol: 2 mol: 30-40 g: 2 mol: 10-15 g: 1500 mL; In the above reaction, the unsaturated amide-ester intermediate converts the phenolic hydroxyl group into a methoxy group under the catalytic action of butyl bromide and potassium carbonate, and then the secondary amine structure on the unsaturated amide-ester intermediate and 3-chloropropyltrimethoxysilane undergo a substitution reaction, and the silane coupling agent is grafted onto the unsaturated amide-ester intermediate. The structural formula of the anti-aging enhancer is shown as follows:

[0008] Preparation of an aging-resistant insulating cable material: Step S1: adding polyvinyl chloride resin, anti-aging enhancer, plasticizer, flame retardant, aluminum nitride, antioxidant, light stabilizer, heat stabilizer and lubricant to a mixer, controlling the stirring rate to 1500-2000 r / min, heating to 100° C., and mixing for 1 hour to obtain a polyvinyl chloride blank; Step S2: putting the polyvinyl chloride ingredients into a twin-screw extruder, adjusting the temperature of each zone of the twin-screw to 100-110°C, 120-130°C, 140-150°C, 160-180°C, 180-190°C, 190-210°C, 190-210°C, 170-180°C, applying 70-80r / min, and an extrusion mass flow rate of 30-40kg / h, melt blending, extrusion, and granulation, and then injection molding by an injection molding machine at 180°C to obtain an aging-resistant insulating cable material.

[0009] Beneficial effects of the present invention: The invention discloses an aging-resistant insulating cable material, which takes polyvinyl chloride as a matrix and is mixed with an anti-aging reinforcing agent. Compared with the existing polyvinyl chloride, the anti-aging agent has better aging resistance. The anti-aging agent is prepared by reacting 2-nitro-diphenol and oleic acid, then adding sodium sulfide for reduction and reacting with 2,5-dihydroxyterephthalic acid, and finally converting the phenolic hydroxyl group into a methoxy group under alkaline conditions, and performing a substitution reaction between a secondary amine structure and 3-chloropropyltrimethoxysilane to obtain an anti-aging reinforcing agent with a silane coupling agent structure. The silane coupling agent structure in the anti-aging reinforcing agent can be coupled with aluminum nitride. When ultraviolet light energy acts on the polyvinyl chloride matrix, the aluminum nitride with a high thermal conductivity can dissipate heat, thereby inhibiting the photodegradation effect of ultraviolet light energy on the polyvinyl chloride matrix, further improving its aging resistance, and at the same time The butoxy group in the anti-aging enhancer serves as an adsorption site for HCl, and can adsorb HCl produced by the photodegradation of polyvinyl chloride, thereby inhibiting the catalytic effect of HCl on the photodegradation of polyvinyl chloride matrix; and the unsaturated double bonds in the anti-aging enhancer can undergo addition reaction with the diene structure produced by the photodegradation of PVC, which can reduce the number of conjugated dienes produced by chain dehydrogenation, and on the other hand, can cross-link with the polyvinyl chloride matrix to form a network structure, effectively improving the mechanical strength of the PVC matrix and reinforcing the aging resistance of the polyvinyl chloride matrix; and the multiple long alkyl chains in the anti-aging enhancer can entangle with the molecular chains of the polyvinyl chloride matrix to form an interpenetrating network, effectively inhibiting the migration ability of the anti-aging enhancer under the action of ultraviolet light energy, and further reinforcing the aging resistance of the polyvinyl chloride matrix under long-term ultraviolet light irradiation. DETAILED DESCRIPTION

[0010] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0011] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 200 r / min, the temperature was raised to 60°C, and the mixture was stirred for 3 hours, and then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the amount ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 2 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and mix them into a reactor, control the stirring reaction rate to 300r / min, heat to 50°C, stir and react for 1h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 60°C, stir and react for 3h, and then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:30g:1mol:4g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and mix them into a reactor, control the stirring reaction rate to 350r / min, heat to 80°C, stir and react for 2h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 1h, then extract with ethyl acetate 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol: 2mol: 30g: 2mol: 10g: 1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin (polyvinyl chloride of Shanghai Aladdin Biochemical Technology Co., Ltd., model P107107) , 15 parts of anti-aging enhancer, 20 parts of plasticizer (plasticizer of Jiangsu Sendi Chemical Technology Co., Ltd.) , 25 parts of flame retardant (tritolyl phosphate) , 3 parts of aluminum nitride, 2 parts of antioxidant (antioxidant 1010) , 2 parts of light stabilizer (UV-531) , 2 parts of heat stabilizer (zinc stearate) , 1 part of lubricant (calcium stearate) , 1 part of lubricant (calcium stearate) , 15 parts of anti-aging enhancer, 20 parts of plasticizer (plasticizer of Jiangsu Sendi Chemical Technology Co., Ltd.) , 25 parts of flame retardant (tritolyl phosphate) , 3 parts of aluminum nitride, 2 parts of antioxidant (antioxidant 1010) , 2 parts of light stabilizer (UV-531) , 2 parts of heat stabilizer (zinc stearate) , 1 part of lubricant (calcium stearate) , 1500 r / min stirring speed, 100°C heating, 1 h mixing to obtain polyvinyl chloride blank; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 100℃, 120℃, 140℃, 160℃, 180℃, 190℃, 190℃, and 170℃, apply 70r / min, and the extrusion mass flow rate is 30kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material. Example

[0012] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 220 r / min, the temperature was raised to 62°C, and the mixture was stirred for reaction for 3.5 hours, and then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the amount ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 2.2 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and mix them into a reactor, control the stirring reaction rate to 320r / min, heat to 52°C, stir and react for 1.5h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 62°C, stir and react for 3.5h, and then vacuum evaporate to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:32g:1mol:4.5g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and mix them into a reactor, control the stirring reaction rate to 400r / min, heat to 82°C, stir and react for 2.5h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 1.5h, then extract with ethyl acetate for 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol:2mol:32g:2mol:11g:1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin, 16 parts of anti-aging enhancer, 22 parts of plasticizer, 26 parts of flame retardant, 4 parts of aluminum nitride, 3 parts of antioxidant, 2 parts of light stabilizer, 3 parts of heat stabilizer and 1.1 parts of lubricant were mixed and added into a mixer, the stirring speed was controlled to be 1600 r / min, the temperature was raised to 100°C, and the polyvinyl chloride blank was obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 105°C, 125°C, 145°C, 165°C, 185°C, 195°C, 200°C, and 175°C, apply 70r / min, and the extrusion mass flow rate is 30kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180°C to obtain aging-resistant insulating cable material. Example

[0013] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added to a reactor, the stirring reaction rate was controlled to be 240 r / min, the temperature was raised to 64°C, and the mixture was stirred for 4 hours, then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the amount ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 2.4 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and add them into the reactor, control the stirring reaction rate to 340r / min, heat to 54°C, stir and react for 2h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 64°C, stir and react for 4h, then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:34g:1mol:5g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and add them into a reactor, control the stirring reaction rate to 450r / min, heat to 84°C, stir and react for 3h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 2h, then extract with ethyl acetate 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol: 2mol: 34g: 2mol: 12g: 1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin, 17 parts of anti-aging enhancer, 24 parts of plasticizer, 27 parts of flame retardant, 5 parts of aluminum nitride, 3 parts of antioxidant, 3 parts of light stabilizer, 2 parts of heat stabilizer and 1.2 parts of lubricant were mixed and added into a mixer, the stirring speed was controlled to be 1700 r / min, the temperature was raised to 100°C, and the polyvinyl chloride blank was obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 110℃, 130℃, 150℃, 170℃, 190℃, 200℃, 200℃, and 180℃, apply 75r / min, and the extrusion mass flow rate is 35kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material. Example

[0014] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 260r / min, the temperature was raised to 66°C, and the mixture was stirred for 4 hours, then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the dosage ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 2.6 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and mix them into a reactor, control the stirring reaction rate to 360r / min, heat to 56°C, stir and react for 2h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 66°C, stir and react for 4h, and then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:36g:1mol:5.5g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and add them into a reactor, control the stirring reaction rate to 450r / min, heat to 86°C, stir and react for 3.5h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 2h, then extract with ethyl acetate 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol: 2mol: 36g: 2mol: 13g: 1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin, 18 parts of anti-aging enhancer, 26 parts of plasticizer, 28 parts of flame retardant, 5 parts of aluminum nitride, 3 parts of antioxidant, 3 parts of light stabilizer, 3 parts of heat stabilizer and 1.3 parts of lubricant were mixed and added into a mixer, the stirring speed was controlled to be 1800 r / min, the temperature was raised to 100° C., and the polyvinyl chloride blank was obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 110℃, 130℃, 150℃, 175℃, 190℃, 205℃, 205℃, and 180℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material. Example

[0015] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 280r / min, the temperature was raised to 68°C, and the mixture was stirred for 4 hours, then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the dosage ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 2.8 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and add them into the reactor, control the stirring reaction rate to 380r / min, heat to 58°C, stir and react for 2h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 68°C, stir and react for 4h, and then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:38g:1mol:6g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and mix them into a reactor, control the stirring reaction rate to 450r / min, heat to 88°C, stir and react for 4h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 2h, then extract with ethyl acetate 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol: 2mol: 38g: 2mol: 14g: 1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin, 19 parts of anti-aging enhancer, 28 parts of plasticizer, 29 parts of flame retardant, 5 parts of aluminum nitride, 3 parts of antioxidant, 3 parts of light stabilizer, 3 parts of heat stabilizer and 1.3 parts of lubricant were mixed and added into a mixer, the stirring rate was controlled to be 1900 r / min, the temperature was raised to 100° C., and the polyvinyl chloride blank was obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 110℃, 130℃, 150℃, 180℃, 190℃, 210℃, 210℃, 180℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material. Example

[0016] The specific implementation process of preparing an aging-resistant insulating cable material in this embodiment is as follows: 1) Preparation of anti-aging enhancer a1: 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 300 r / min, the temperature was raised to 70°C, and the mixture was stirred for 4 hours, then washed with water 3 times and dried to obtain an unsaturated ester intermediate; in the above reaction, the amount ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF was 1 mol: 2 mol: 3 g: 500 mL; a2: Take the unsaturated ester intermediate, sodium sulfide and ethanol and add them into the reactor, control the stirring reaction rate to 400r / min, heat to 60°C, stir and react for 2h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 66°C, stir and react for 4h, and then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; in the above reaction, the amount ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2mol:40g:1mol:6g:1000mL; a3: Take unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate and DMF and add them into a reactor, control the stirring reaction rate to 450r / min, heat to 90°C, stir and react for 4h, then add 3-chloropropyltrimethoxysilane and triethylamine, continue to react for 2h, then extract with ethyl acetate 3 times, then extract the ethyl acetate phase with water, and finally evaporate in vacuum to obtain an anti-aging enhancer; in the above reaction, the amount ratio of unsaturated amide-ester intermediate, bromobutyl, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1mol: 2mol: 40g: 2mol: 15g: 1500mL; 2) Preparation of aging-resistant insulating cable materials s1: 100 parts of polyvinyl chloride resin, 20 parts of anti-aging enhancer, 30 parts of plasticizer, 30 parts of flame retardant, 5 parts of aluminum nitride, 3 parts of antioxidant, 3 parts of light stabilizer, 3 parts of heat stabilizer and 1.5 parts of lubricant were mixed and added into a mixer, the stirring speed was controlled to be 2000 r / min, the temperature was raised to 100°C, and the polyvinyl chloride blank was obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 110℃, 130℃, 150℃, 180℃, 190℃, 210℃, 210℃, 180℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material.

[0017] Comparative Example 1 The specific implementation process of preparing an aging-resistant insulating cable material in this comparative example is as follows: s1: 100 parts of polyvinyl chloride resin, 30 parts of plasticizer, 30 parts of flame retardant, 2 parts of silane coupling agent (vinyl trimethoxy silane is selected in this comparative example), 15 parts of aluminum nitride, 3 parts of antioxidant, 3 parts of light stabilizer, 3 parts of heat stabilizer and 1.5 parts of lubricant are mixed and added into a mixer, the stirring speed is controlled to 2000 r / min, the temperature is raised to 100°C, and the polyvinyl chloride blank is obtained after mixing for 1 hour; s2: Put the polyvinyl chloride billet into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 110℃, 130℃, 150℃, 180℃, 190℃, 210℃, 210℃, 180℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blending, extrusion, and granulation are carried out, and then injection molding is carried out by an injection molding machine at 180℃ to obtain aging-resistant insulating cable material.

[0018] Comparative Example 2 s1: The PVC cable material (this comparative example uses the anti-aging insulating and environmentally friendly PVC cable material produced by Foshan Shunde Jupang Plastic Co., Ltd.) is injection molded by an injection molding machine at 180°C to obtain an anti-aging insulating cable material.

[0019] Tensile Strength / Elongation Test: The polyvinyl chloride blanks prepared in Examples 1-6 and Comparative Examples 1-2 were injection molded by an injection molding machine at 200° C., and test specimens were prepared and tested according to GB / T1040.1-2018. Impact strength test: The polyvinyl chloride blanks prepared in Examples 1-6 and Comparative Examples 1-2 were injection molded by an injection molding machine at 200° C., and test specimens were prepared and tested according to GB / T1843-2008 Method A; specific test data are shown in Table 1:

[0020] From the data in Table 1, it can be seen that the tensile strength of the aging-resistant insulating cable materials prepared in Examples 1-6 is 53-60 MPa, the elongation is 511-540%, and the impact strength is 8.54-10.58 KJ / m 2 ; Slightly better than the aging-resistant insulating cable material of Comparative Example 1-2.

[0021] Aging resistance test: The test specimens were placed in a test chamber and subjected to a 2500h UV illumination experiment using UVA-351 according to GB / T16442.3-2022 Method B. Afterwards, the tensile strength / elongation retention rate and impact strength retention rate of the specimens were tested according to GB / T1040.1-2018 and GB / T1843-2008, respectively. The specific test data are shown in Table 2:

[0022] It can be seen from the data in Table 2 that after 2500 hours of ultraviolet light irradiation, the average tensile strength retention rate of the aging-resistant insulating cable materials prepared in Examples 1-6 is 91.7%, the average elongation retention rate is 90.8%, and the average impact strength retention rate is 91.6%. All the data are slightly better than those in Comparative Examples 1-2, indicating that the aging-resistant insulating cable material prepared in this embodiment has excellent anti-aging performance.

[0023] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0024] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An aging-resistant insulating cable material, characterized in that: The composition comprises, by weight, 100 parts of polyvinyl chloride resin, 15-20 parts of anti-aging enhancer, 20-30 parts of plasticizer, 25-30 parts of flame retardant, 3-5 parts of aluminum nitride, 2-3 parts of antioxidant, 2-3 parts of light stabilizer, 2-3 parts of heat stabilizer and 1-1.5 parts of lubricant; Preparation of anti-aging enhancer: Step A1: 2-nitro-diphenol, oleic acid, sodium hydroxide and DMF were mixed and added, the temperature was raised to 60-70° C., stirred for reaction for 3-4 hours, washed with water 3 times and dried to obtain an unsaturated ester intermediate; Step A2: Mix the unsaturated ester intermediate, sodium sulfide and ethanol, heat to 50-60°C, stir to react for 1-2h, then add 2,5-dihydroxyterephthalic acid and DCC, heat to 60-70°C, stir to react for 3-5h, and then evaporate under reduced pressure to obtain the unsaturated amide-ester intermediate; Step A3: Take the unsaturated amide-ester intermediate, butyl bromide, anhydrous potassium carbonate and DMF, mix them, heat to 80-90° C., stir and react for 2-4 hours, then add 3-chloropropyltrimethoxysilane and triethylamine, and continue to react for 1-2 hours to obtain an anti-aging enhancer.

2. The aging-resistant insulating cable material according to claim 1, characterized in that: In step A1, the usage ratio of 2-nitro-meta-diphenol, oleic acid, sodium hydroxide and DMF is 1 mol: 2 mol: 2-3 g: 500 mL.

3. The aging-resistant insulating cable material according to claim 2, characterized in that: In step A2, the usage ratio of the unsaturated ester intermediate, sodium sulfide, 2,5-dihydroxyterephthalic acid, DCC and ethanol is 2 mol: 30-40 g: 1 mol: 4-6 g: 1000 mL.

4. The aging-resistant insulating cable material according to claim 3, characterized in that: In step A3, the usage ratio of the unsaturated amide-ester intermediate, butyl bromide, anhydrous potassium carbonate, 3-chloropropyltrimethoxysilane, triethylamine and DMF is 1 mol: 2 mol: 30-40 g: 2 mol: 10-15 g: 1500 mL.

5. The method for preparing an aging-resistant insulating cable material according to claim 4, characterized in that: The steps include: Step S1: mixing polyvinyl chloride resin, anti-aging enhancer, plasticizer, flame retardant, aluminum nitride, antioxidant, light stabilizer, heat stabilizer and lubricant, and kneading for 1 hour to obtain polyvinyl chloride blank; Step S2: putting the polyvinyl chloride ingredients into a twin-screw extruder, adjusting the temperature of each zone of the twin-screw to 100-110°C, 120-130°C, 140-150°C, 160-180°C, 180-190°C, 190-210°C, 190-210°C, 170-180°C, melt blending, extrusion, and granulation, and then injection molding by an injection molding machine at 180°C to obtain an aging-resistant insulating cable material.

6. The method for preparing an aging-resistant insulating cable material according to claim 5, characterized in that: The mixing temperature was 100°C.

7. The method for preparing an aging-resistant insulating cable material according to claim 6, characterized in that: The flame retardant is tricresyl phosphate.

8. The method for preparing an aging-resistant insulating cable material according to claim 6, characterized in that: The light stabilizer is UV-531.