High-viscosity high-elasticity asphalt modified additive and preparation method thereof

A high-viscosity and high-elastic asphalt modification additive, comprising styrene-butadiene-styrene block copolymer and other components, addresses the limitations of existing additives by enhancing asphalt's performance in extreme temperatures and wear resistance, ensuring durability and effective water management.

CN119081337AInactive Publication Date: 2024-12-06SHANGHAI XIONGWEN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411256255.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing asphalt modification additives exhibit poor cold resistance, high temperature resistance, anti-leakage effect, and wear resistance, leading to issues such as peeling, shifting, and low bonding strength with underlying layers.

Method used

A high-viscosity and high-elastic asphalt modification additive composed of styrene-butadiene-styrene block copolymer, C9 petroleum resin, polyolefin elastomer, polyethylene, grafting agent, lubricant, dispersant, and rubber softener, prepared through a specific mixing and granulation process.

Benefits of technology

The additive enhances asphalt's viscosity and elasticity, providing resistance to extreme temperatures, reducing friction and noise, improving wear resistance, and facilitating water seepage, thereby extending the pavement's service life and maintaining road integrity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-viscosity and high-elasticity asphalt modification additive, which at least solves the technical problem of poor use effect of the asphalt modification additive in the prior art, and comprises the following components by mass: 45-55% of styrene-butadiene-styrene block copolymer; 5-12% of C9 petroleum resin; 4-8% of a polyolefin elastomer and 6-12% of polyethylene; 2-8% of a grafting agent; 1-2% of a lubricant; 1-2% of a dispersant; and 15-22% of a rubber softening agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a high-viscosity and high-elastic asphalt modified additive and a preparation method thereof, and belongs to the technical field of pavement construction. Background Art

[0002] The paving and preventive maintenance of asphalt pavements in roads, bridges, tunnels, airports, etc. can improve and restore the surface function of the pavement, reduce the number of repairs during the entire life cycle, and extend the service life of the pavement. It has been widely used in my country. Asphalt pavements require good bonding and wear resistance with the underlying layer. Due to the low viscosity of asphalt, low bonding strength between the overlay and the old pavement, or low wear resistance of the overlay, it is easy to fall off, peel off, shift, loosen and other diseases. Therefore, the research on high-viscosity modified asphalt materials has received widespread attention.

[0003] Existing asphalt modification additives have poor cold resistance, poor high temperature resistance, poor anti-leakage effect, and cannot achieve high wear resistance. Summary of the invention

[0004] The present application provides a high-viscosity and high-elastic asphalt modification additive to at least solve the technical problem of poor use effect of asphalt modification additives in the prior art.

[0005] In order to achieve the above-mentioned purpose, the present application provides a high-viscosity and high-elastic asphalt modification additive, which comprises, by mass component ratio:

[0006] Styrene-butadiene-styrene block copolymer: 45-55%

[0007] C9 petroleum resin: 5-12%

[0008] Polyolefin elastomer: 4-8%

[0009] Polyethylene: 6-12%

[0010] Grafting agent: 2-8%

[0011] Lubricant: 1-2%

[0012] Dispersant: 1-2%

[0013] Rubber softener 15-22%.

[0014] Preferably, the components by mass ratio include:

[0015] Styrene-butadiene-styrene block copolymer: 50%

[0016] C9 petroleum resin: 8%

[0017] Polyolefin elastomer: 5%

[0018] Polyethylene: 10%

[0019] Grafting agent 5%

[0020] Lubricant 1.5%

[0021] Dispersant 1.5%

[0022] Rubber softener 19%.

[0023] Preferably, the grafting agent is maleic anhydride or maleic anhydride or dicumyl peroxide.

[0024] Preferably, the lubricant is at least one of erucamide, stearic acid amide, vinyl bisstearamide, oleic acid amide, butadiene-styrene copolymer, and polyethylene wax.

[0025] Preferably, the dispersant is at least one of ethanol, hexadecyltrimethylammonium bromide and polysulfonic acid.

[0026] Preferably, the rubber softener is naphthenic oil or dioctyl phthalate or a mixture of the two.

[0027] The present application also relates to a method for preparing a high-viscosity and high-elastic asphalt modified additive, comprising the following steps:

[0028] Step 1: premix the styrene-butadiene-styrene block copolymer and the rubber softener in proportion, heat to 30-80 degrees, rotate at 200-300 rpm, and rotate for 10-30 minutes until the styrene-butadiene-styrene block copolymer is completely expanded, thus completing the first mixing;

[0029] Step 2: Then add polyethylene and grafting agent for second mixing, the temperature is 30-60 degrees, the speed is 100-150 rpm, and the second mixing is completed for 5-15 minutes;

[0030] Step 3, add C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant and blend for 3-8 minutes, discharge and cool;

[0031] Step 4: granulate the cooled material, and control the temperature of the granulator at 120-200 degrees and the speed at 300-400 rpm.

[0032] Preferably, in the step 1, the styrene-butadiene-styrene block copolymer and the rubber softener are put into a ribbon mixer in proportion for premixing, heated to 50 degrees, rotated at 200-300 rpm, and rotated for 20 minutes until the styrene-butadiene-styrene block copolymer is completely expanded, thereby completing the first mixing.

[0033] Preferably, in the step 2, polyethylene and grafting agent are added for a second mixing, the temperature is 45 degrees, the rotation speed is 100-150 rpm, and the second mixing is completed in 10 minutes.

[0034] Preferably, in the step three, C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant are blended for 5 minutes, and the mixture is discharged for cooling.

[0035] Preferably, in the step 4, the cooled material is put into the hopper of a parallel twin-screw granulator for granulation, and the temperature of the granulator is controlled at 150 degrees and the speed is controlled at 350 revolutions per minute.

[0036] Preferably, the method further comprises step 5, wherein the rotation speed of the pelletizer is controlled to a particle size of about 3 MM according to the on-site conditions, and the pellets are sieved and bagged before leaving the factory.

[0037] According to the above content, the beneficial effects of this application are:

[0038] The high-viscosity and high-elasticity asphalt modified additive prepared by the present application has the following advantages: it can make the asphalt highly viscous and resistant to severe cold, and the road surface will not become brittle or crack in an environment of minus 30 degrees; it has high elasticity, can absorb stress, extend the service life, does not produce dust, reduce friction resistance, and reduce noise; it is conducive to leakage, and the skeleton stone aggregate can form a beam-like network structure to allow road surface water to seep into the ground in a short time, keeping the road surface dry; it is resistant to high temperature and high wear resistance. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated in conjunction with the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application. In addition, it can also be understood that although the efforts made in this development process may be complex and lengthy, for ordinary technicians in the field related to the contents disclosed in the present application, some designs, manufacturing or production changes based on the technical contents disclosed in the present application are only conventional technical means, and should not be understood as insufficient contents disclosed in the present application.

[0040] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those of ordinary skill in the art that the embodiments described in this application may be combined with other embodiments without conflict.

[0041] Unless otherwise defined, the technical terms or scientific terms involved in this application should be understood by people with ordinary skills in the technical field to which this application belongs. The words "one", "a", "a", "the" and the like involved in this application do not indicate a quantitative limitation, and may represent the singular or plural. The terms "include", "comprise", "have" and any of their variations involved in this application are intended to cover non-exclusive inclusions; for example, a process, method, system, product or device that includes a series of steps or modules (units) is not limited to the listed steps or units, but may also include steps or units that are not listed, or may also include other steps or units inherent to these processes, methods, products or devices. The words "connect", "connected", "coupled" and the like involved in this application are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. The "multiple" involved in this application refers to greater than or equal to two. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, "A and / or B" can represent: A exists alone, A and B exist at the same time, and B exists alone. The terms "first", "second", "third" and the like involved in the present application are merely used to distinguish similar objects and do not represent a specific ordering of the objects.

[0042] The present application relates to a high-viscosity and high-elastic asphalt modification additive, which comprises, by mass component ratio:

[0043] Styrene-butadiene-styrene block copolymer (SBS): 45-55%

[0044] C9 petroleum resin: 5-12%

[0045] Polyolefin elastomer (POE): 4-8%

[0046] Polyethylene (PE): 6-12%

[0047] Grafting agent: 2-8%

[0048] Lubricant: 1-2%

[0049] Dispersant: 1-2%

[0050] Rubber softener 15-22%.

[0051] The present application also relates to a method for preparing the above-mentioned high-viscosity and high-elastic asphalt modification additive, comprising the following steps:

[0052] Step 1: premix the styrene-butadiene-styrene block copolymer and the rubber softener in proportion, heat to 30-80 degrees and rotate at 200-300 rpm for 10-30 minutes until the styrene-butadiene-styrene block copolymer is completely expanded, thus completing the first mixing;

[0053] Step 2: Then add polyethylene and grafting agent for second mixing, the temperature is 30-60 degrees, the speed is 100-150 rpm, and the second mixing is completed in 5-15 minutes;

[0054] Step 3, add C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant and blend for 3-8 minutes, discharge and cool;

[0055] Step 4: granulate the cooled material, and control the temperature of the granulator at 120-200 degrees and the speed at 300-400 rpm.

[0056] The technical solution of the present application is further described below through specific embodiments.

[0057] Embodiment 1

[0058] In this embodiment, the high-viscosity and high-elastic asphalt modification additive includes the following components by mass ratio:

[0059] Styrene-butadiene-styrene block copolymer: 50%

[0060] C9 petroleum resin: 8%

[0061] Polyolefin elastomer: 5%

[0062] Polyethylene: 10%

[0063] Grafting agent 5%

[0064] Lubricant 1.5%

[0065] Dispersant 1.5%

[0066] Rubber softener 19%.

[0067] The grafting agent is maleic anhydride density.

[0068] The lubricant is erucamide.

[0069] The dispersant is ethanol.

[0070] The rubber softener is a mixture of naphthenic oil and dioctyl phthalate.

[0071] The preparation method of the above-mentioned high-viscosity and high-elastic asphalt modification additive comprises the following steps:

[0072] Step 1: Add SBS and rubber softener in proportion into a ribbon mixer for premixing, heat to 50 degrees and rotate at 300 rpm for 20 minutes until SBS is completely expanded, thus completing the first mixing.

[0073] Step 2: Add polyethylene and grafting agent for second mixing at a temperature of 45 degrees and a rotation speed of 100 rpm for 10 minutes.

[0074] Step 3, C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant are blended for 5 minutes, and the mixture is discharged for cooling.

[0075] Step 4: put the cooled material into the hopper of a parallel twin-screw granulator for granulation. The temperature of the granulator is controlled at 150 degrees and the speed is controlled at 350 rpm.

[0076] Step 5: The pelletizer speed is controlled according to the on-site situation to keep the particle size at about 3MM, and the pellets are sieved and bagged before leaving the factory.

[0077] The high-viscosity and high-elastic asphalt modified additive prepared by this application has the following advantages:

[0078] 1. It is resistant to severe cold and has high viscosity. The road surface will not become brittle or crack in an environment of minus 30 degrees.

[0079] 2. High elasticity, can absorb stress, extend service life, no dust, reduce friction resistance and noise.

[0080] 3. It is beneficial to seepage. The skeleton stone aggregate can form a beam-like network structure to allow the surface water on the road to seep into the ground in a short time, keeping the road surface dry and reducing accidents.

[0081] 4. High temperature resistant, it does not soften at a high temperature of 50 degrees, thus avoiding the melting of asphalt on ordinary asphalt pavement in summer.

[0082] 5. High wear resistance.

[0083] Embodiment 2

[0084] In this embodiment, the high-viscosity and high-elastic asphalt modification additive includes the following components by mass ratio:

[0085] Styrene-butadiene-styrene block copolymer: 45%

[0086] C9 petroleum resin: 12%

[0087] Polyolefin elastomer: 8%

[0088] Polyethylene: 12%

[0089] Grafting agent 6%

[0090] Lubricant 1%

[0091] Dispersant 1%

[0092] Rubber softener 15%.

[0093] The grafting agent is maleic anhydride.

[0094] The lubricant is stearic acid amide.

[0095] The dispersant is at least one of cetyltrimethylammonium bromide.

[0096] The rubber softener is naphthenic oil.

[0097] The preparation method of the above-mentioned high-viscosity and high-elastic asphalt modification additive comprises the following steps:

[0098] Step 1: Add SBS and rubber softener in proportion into a ribbon mixer for premixing, heat to 80 degrees and rotate at 250 rpm for 15 minutes to complete the first mixing.

[0099] Step 2: Add polyethylene and grafting agent for second mixing at a temperature of 45 degrees and a rotation speed of 150 rpm for 15 minutes.

[0100] Step 3, C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant are blended for 5 minutes, and the mixture is discharged for cooling.

[0101] Step 4: put the cooled material into the hopper of a parallel twin-screw granulator for granulation. The temperature of the granulator is controlled at 150 degrees and the speed is controlled at 350 rpm.

[0102] Step 5: The pelletizer speed is controlled according to the on-site situation to keep the particle size at about 3MM, and the pellets are sieved and bagged before leaving the factory.

[0103] Embodiment 3

[0104] In this embodiment, the high-viscosity and high-elastic asphalt modification additive includes the following components by mass ratio:

[0105] Styrene-butadiene-styrene block copolymer: 55%

[0106] C9 petroleum resin: 5%

[0107] Polyolefin elastomer: 4%

[0108] Polyethylene: 6%

[0109] Grafting agent 4%

[0110] Lubricant 2%

[0111] Dispersant 2%

[0112] Rubber softener 22%.

[0113] The grafting agent is dicumyl peroxide.

[0114] The lubricant is a mixture of stearic acid amide, vinyl bisstearic acid amide, oleic acid amide, butadiene-styrene copolymer and polyethylene wax.

[0115] The dispersant is polysulfonic acid.

[0116] The rubber softener is dioctyl phthalate.

[0117] The preparation method of the above-mentioned high-viscosity and high-elastic asphalt modification additive comprises the following steps:

[0118] Step 1: Add SBS and rubber softener in proportion into a ribbon mixer for premixing, heat to 30 degrees and rotate at 200 rpm for 30 minutes until SBS is completely expanded, thus completing the first mixing.

[0119] Step 2: Add polyethylene and grafting agent for second mixing at a temperature of 45 degrees and a rotation speed of 120 rpm for 10 minutes.

[0120] Step 3, C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant are blended for 5 minutes, and the mixture is discharged for cooling.

[0121] Step 4: put the cooled material into the hopper of a parallel twin-screw granulator for granulation. The temperature of the granulator is controlled at 120 degrees and the speed is controlled at 300 revolutions per minute.

[0122] Step 5: The pelletizer speed is controlled according to the on-site situation to keep the particle size at about 3MM, and the pellets are sieved and bagged before leaving the factory.

[0123] In other embodiments, the grafting agent may also be a mixture of two or more of maleic anhydride, maleic anhydride, and dicumyl peroxide. The lubricant may be a mixture of two or more of erucic acid amide, stearic acid amide, vinyl bisstearic acid amide, oleic acid amide, butadiene-styrene copolymer, and polyethylene wax. The dispersant may be two or more of ethanol, hexadecyltrimethylammonium bromide, and polysulfonic acid. The rubber softener may be one of naphthenic oil and dioctyl phthalate.

[0124] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. High-viscosity and high-elastic asphalt modification additive, characterized in that: The components by mass ratio include: Styrene-butadiene-styrene block copolymer: 45-55% C9 petroleum resin: 5-12% Polyolefin elastomer: 4-8% Polyethylene: 6-12% Grafting agent: 2-8% Lubricant: 1-2% Dispersant: 1-2% Rubber softener 15-22%.

2. The high-viscosity and high-elastic asphalt modification additive according to claim 1, characterized in that: The components by mass ratio include: Styrene-butadiene-styrene block copolymer: 50% C9 petroleum resin: 8% Polyolefin elastomer: 5% Polyethylene: 10% Grafting agent 5% Lubricant 1.5% Dispersant 1.5% Rubber softener 19%.

3. The high-viscosity and high-elastic asphalt modification additive according to claim 1 or 2, characterized in that: The grafting agent is maleic anhydride or maleic anhydride or dicumyl peroxide.

4. The high-viscosity and high-elastic asphalt modification additive according to claim 1 or 2, characterized in that: The lubricant is at least one of erucamide, stearic acid amide, vinyl bisstearic acid amide, oleic acid amide, butadiene-styrene copolymer, and polyethylene wax.

5. The high-viscosity and high-elastic asphalt modification additive according to claim 1 or 2, characterized in that: The dispersant is at least one of ethanol, hexadecyltrimethylammonium bromide and polysulfonic acid.

6. The high-viscosity and high-elastic asphalt modification additive according to claim 1 or 2, characterized in that: The dispersant is at least one of ethanol, hexadecyltrimethylammonium bromide and polysulfonic acid.

7. The high-viscosity and high-elastic asphalt modification additive according to claim 1 or 2, characterized in that: The rubber softener is naphthenic oil or dioctyl phthalate or a mixture of the two.

8. A method for preparing a high-viscosity and high-elastic asphalt modification additive, characterized in that: The following steps are involved: Step 1: premix the styrene-butadiene-styrene block copolymer and the rubber softener in proportion, heat to 30-80 degrees, rotate at 200-300 rpm for 10-30 minutes, until the styrene-butadiene-styrene block copolymer is completely expanded, thus completing the first mixing; Step 2: Add polyethylene and grafting agent for second mixing at a temperature of 30-60 degrees and a rotation speed of 100-150 rpm for 5-15 minutes to complete the second mixing; Step 3: Add C9 petroleum resin, polyethylene, polyolefin elastomer, lubricant and dispersant and blend for 3-8 minutes, then discharge and cool; Step 4: granulate the cooled material, and control the temperature of the granulator at 120-200 degrees and the speed at 300-400 rpm.

9. The method for preparing the high-viscosity and high-elastic asphalt modification additive according to claim 8, characterized in that: In the step 1, the styrene-butadiene-styrene block copolymer and the rubber softener are put into a ribbon mixer in proportion for premixing, heated to 50 degrees and rotated at 200-300 rpm for 20 minutes until the styrene-butadiene-styrene block copolymer is completely expanded, thus completing the first mixing.

10. The method for preparing the high-viscosity and high-elastic asphalt modification additive according to claim 8, characterized in that: In the step 2, polyethylene and grafting agent are added for a second mixing, the temperature is 45 degrees, the rotation speed is 100-150 rpm, and the second mixing is completed in 10 minutes.