ABS-PVC alloy material and preparation method thereof

By optimizing the component ratio and process flow in ABS-PVC alloy materials, the problems of low surface gloss and heavy specific gravity are solved, and ABS-PVC alloy materials with high gloss, low specific gravity and high toughness are achieved, satisfying a variety of Application requirements and reduce costs.

CN119081343APending Publication Date: 2024-12-06HUNAN HONGDE NEW MATERIALS CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411472547.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ABS-PVC alloy materials have problems of low surface gloss and heavy specific gravity, which is difficult to meet the application needs of high gloss and low specific gravity.

Method used

50 to 70 parts of ABS resin, 20 to 40 parts of PVC resin, 5 to 10 parts of AS resin, 4 to 10 parts of compatible toughener, 1 to 5 parts of flame retardant, 0.1 to 0.4 parts of gloss agent, and 0.1 lubricant are used. A combination of ~0.5 parts, 0.1 to 0.5 parts of antioxidant and 0.1 to 0.3 parts of stabilizer was prepared by high-speed stirring and twin-screw extrusion granulation process to prepare an ABS-PVC alloy material with high gloss and low specific gravity.

Benefits of technology

It reduces the use of flame retardants, reduces the specific gravity of alloy materials, improves the toughness and surface gloss of the materials, meets the requirements of automotive interiors and home appliance exterior parts, and saves material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081343A_ABST
    Figure CN119081343A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of alloy materials, and discloses an ABS-PVC alloy material and a preparation method thereof, and the ABS-PVC alloy material comprises the following components in parts by weight: 50-70 parts of ABS resin, 20-40 parts of PVC resin, 5-10 parts of AS resin, 4-10 parts of a compatible flexibilizer, 1-5 parts of a flame retardant, 0.1-0.4 part of a gloss agent, 0.1-0.5 part of a lubricant, 0.1-0.5 part of an antioxidant and 0.1-0.3 part of a stabilizer. The ABS-PVC alloy material disclosed by the invention has the advantages of light specific gravity, low material cost, high toughness, high glossiness and good flame-retardant effect, and can meet the requirements of many automobile interiors and household appliance appearance parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy materials, and in particular to an ABS-PVC alloy material and a preparation method thereof. Background Art

[0002] Polyvinyl chloride (PVC) and acrylonitrile-butadiene-styrene copolymer (ABS) are two polymer materials widely used in industry and life. PVC is widely used due to its excellent insulation, flame retardancy and chemical corrosion resistance; while ABS is favored for its good mechanical properties, impact resistance and processing performance. However, the use of only PVC or ABS materials is often difficult to meet the complex and changing application requirements. Therefore, the development of an ABS-PVC alloy material that has the excellent properties of both is of great significance for broadening the application field of the material and improving the comprehensive performance of the material.

[0003] At present, high gloss materials have broad application prospects in the fields of decoration, furniture and automobile interior. For ABS-PVC alloy materials, it is not only required to have good mechanical properties and flame retardant properties, but also required to have light specific gravity and high surface gloss. Existing ABS-PVC alloy materials, such as the fluid PVC / ABS alloy material disclosed in Chinese patent CN102453306B, use a large amount of flame retardant antimony trioxide, which weakens the surface gloss to a certain extent and increases the specific gravity of the alloy material itself.

[0004] Therefore, there is an urgent need to develop an ABS-PVC alloy material with good flame retardant effect, high mechanical properties, light specific gravity and high surface gloss. Summary of the invention

[0005] The main purpose of the present invention is to provide an ABS-PVC alloy material and a preparation method thereof, aiming to solve the technical problems of low surface gloss and heavy specific gravity of the existing ABS-PVC alloy material.

[0006] To achieve the above objectives, in a first aspect, the present invention provides an ABS-PVC alloy material, comprising the following components in parts by weight: 50 to 70 parts of ABS resin, 20 to 40 parts of PVC resin, 5 to 10 parts of AS resin, 4 to 10 parts of compatible toughening agent, 1 to 5 parts of flame retardant, 0.1 to 0.4 parts of gloss agent, 0.1 to 0.5 parts of lubricant, 0.1 to 0.5 parts of antioxidant and 0.1 to 0.3 parts of stabilizer.

[0007] Preferably, the ABS resin is a compound of a bulk ABS resin and an emulsion ABS resin, and the weight ratio of the bulk ABS resin to the emulsion ABS resin is 1:(2-3).

[0008] Preferably, the degree of polymerization of the PVC resin is 500.

[0009] Preferably, the compatible toughening agent is at least one of chlorinated polyethylene, ethylene vinyl acetate copolymer, methyl methacrylate-butadiene-styrene copolymer and nitrile rubber.

[0010] Preferably, the flame retardant is a compound of chlorinated polyethylene and antimony trioxide.

[0011] Preferably, the brightener is at least one of a basic heavy metal and an amide compound.

[0012] Preferably, the lubricant is a pentaerythritol stearate lubricant.

[0013] Preferably, the antioxidant is a compound of a hindered phenol antioxidant and a phosphite antioxidant.

[0014] Preferably, the stabilizer is at least one of an organic tin heat stabilizer, a lead salt heat stabilizer and a rare earth heat stabilizer.

[0015] In a second aspect, the present invention further provides a method for preparing the ABS-PVC alloy material of the first aspect, comprising:

[0016] Weigh ABS resin, PVC resin, AS resin, compatible toughening agent, flame retardant, gloss agent, lubricant, antioxidant and stabilizer according to weight parts;

[0017] After drying, the ABS resin, the PVC resin and the AS resin are fed into a high-speed mixer for high-speed stirring to obtain a first mixed material; wherein the high-speed stirring is controlled at a speed of 900 to 1000 rpm and a control time of 8 to 12 minutes;

[0018] Adding the compatible toughening agent, the flame retardant, the gloss agent, the lubricant, the antioxidant and the stabilizer to the first mixed material, and stirring at a medium-low speed to obtain a second mixed material; wherein the medium-low speed stirring is controlled at a speed of 400 to 800 rpm and the control time is 4 to 8 minutes;

[0019] The second mixed material is fed into a twin-screw extruder for extrusion granulation to obtain an ABS-PVC alloy material.

[0020] The above ABS-PVC alloy material and its preparation method have the following beneficial effects:

[0021] 1) Compared with the existing flame-retardant ABS / PVC materials, the ABS-PVC alloy material of the present invention reduces the use of flame retardants and reduces the specific gravity (or density) of the ABS-PVC alloy material, thereby saving material costs;

[0022] 2) The present invention uses a compatible toughening agent and AS resin to promote the compatibility of ABS resin and PVC resin, thereby improving the toughness of the ABS-PVC alloy material, and uses AS resin for volume expansion and reinforcement, thereby ensuring the tensile and bending strength of the ABS-PVC alloy material; at the same time, the added AS resin also plays a role in increasing the surface gloss;

[0023] 3) The present invention uses a glossing agent to further improve the surface gloss of the ABS-PVC alloy material without affecting the mechanical properties and flame retardant properties of the alloy material, thereby meeting the requirements of many automotive interior and home appliance exterior parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figure is a schematic flow chart of a method for preparing an ABS-PVC alloy material in one embodiment of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] In one embodiment, the present invention provides an ABS-PVC alloy material for automotive interior and home appliance exterior parts, wherein the ABS-PVC alloy material comprises the following components in parts by weight: 50 to 70 parts of ABS resin, 20 to 40 parts of PVC resin, 5 to 10 parts of AS resin, 4 to 10 parts of compatible toughening agent, 1 to 5 parts of flame retardant, 0.1 to 0.4 parts of gloss agent, 0.1 to 0.5 parts of lubricant, 0.1 to 0.5 parts of antioxidant and 0.1 to 0.3 parts of stabilizer.

[0027] Furthermore, the ABS resin is a compound of bulk ABS resin and emulsion ABS resin, and the weight ratio of the bulk ABS resin to the emulsion ABS resin is 1:(2-3).

[0028] In this embodiment, the bulk ABS resin can be selected from the bulk ABS resin with the brand number 8391 produced by Shanghai Gaoqiao; the emulsion ABS resin can be selected from the emulsion ABS resin with the brand number DG-417 produced by Tianjin Dagu.

[0029] Since the bulk ABS resin and the emulsion ABS resin have differences in the synthesis process, the performance of the two will be somewhat different. The rubber particle size of the bulk ABS resin is larger than that of the emulsion ABS resin, and there are more embedded materials in the rubber particles. Therefore, to a certain extent, the impact strength of the bulk ABS resin will be higher than that of the emulsion ABS resin, while the surface gloss is lower than that of the emulsion ABS resin. In this embodiment, the bulk ABS resin and the emulsion ABS resin are compounded to obtain ABS resin, and the compounded ABS resin is used to prepare the PVC-ABS alloy material, and the comprehensive performance of the PVC-ABS alloy material is better.

[0030] Furthermore, the polymerization degree of the PVC resin is 500.

[0031] In this embodiment, the PVC resin can be selected from commercially available PVC resins, and the selected resin only needs to meet the polymerization degree of 500 tested according to the national standard GB / T 5761-2006; the AS resin (i.e., acrylonitrile-styrene resin) can be selected from the AS resin produced by LG Yongxing with a grade of 80-HF and a glossiness of 85GU.

[0032] The polar activity of the C-Cl segment in PVC resin will be affected by the AN (C≡N) polar segment in ABS resin and AS resin. The C-Cl segment plays an important role in the entire conformation. As the amount of acrylonitrile (AN) in ABS resin increases, the density of the C≡N polar group increases, making the ABS resin and PVC resin dispersed with each other and evenly forming good compatibility. However, acrylonitrile cannot be continuously increased. When acrylonitrile is excessive, the movement of the segment is hindered, thereby reducing the compatibility. At the same time, the surface gloss of styrene (St) in AS resin increases with the increase of its content.

[0033] Furthermore, the compatible toughening agent is at least one of chlorinated polyethylene (CPE), ethylene vinyl acetate copolymer (EVA), methyl methacrylate-butadiene-styrene copolymer (MBS) and nitrile rubber (NBR).

[0034] In this embodiment, the chlorinated polyethylene can be selected from the chlorinated polyethylene with the brand name 135A produced by Rizhao Samsung Chemical; the ethylene vinyl acetate copolymer can be selected from the commercially available ethylene vinyl acetate copolymer; the methyl methacrylate-butadiene-styrene copolymer can be selected from the methyl methacrylate-butadiene-styrene copolymer with the brand name EM500 produced by LG of South Korea; and the nitrile rubber can be selected from the nitrile rubber with the brand name GM50 produced by Kanggaote.

[0035] Furthermore, the flame retardant is a compound of chlorinated polyethylene (CPE) and antimony trioxide.

[0036] In this embodiment, the weight ratio of chlorinated polyethylene to antimony trioxide in the flame retardant is 15:1, and antimony trioxide can be antimony trioxide produced by Jinan Taixing Fine Chemical Co., Ltd.

[0037] Chlorinated polyethylene can be used as a compatibility toughening agent and flame retardant at the same time. On the one hand, adding chlorinated polyethylene can promote the compatibility of ABS resin and PVC resin and improve the toughness of the alloy material. On the other hand, it can greatly reduce the use of flame retardants, especially the antimony trioxide content in the flame retardant, which can reduce costs while having good flame retardant properties. It should be noted that the addition of chlorinated polyethylene can improve the toughness and elasticity of the product, but it will reduce the tensile and bending strength. At this time, adding AS resin can not only promote the compatibility of ABS resin and PVC resin, but also play a reinforcing role.

[0038] Furthermore, the brightener is at least one of a basic heavy metal and an amide compound.

[0039] In this embodiment, the basic heavy metal can be selected from the basic heavy metal with the brand name CP110 produced by Zhuhai Lianding Chemical; the amide compound can be selected from the amide compound with the brand name 222 produced by Qingdao Sino Chemical. Preferably, when the brightener is a mixture of the basic heavy metal and the amide compound, the weight ratio of the basic heavy metal to the amide compound is 1:1.

[0040] Furthermore, the lubricant is a pentaerythritol stearate lubricant.

[0041] In this embodiment, the pentaerythritol stearate can be commercially available pentaerythritol stearate with the brand name PETS.

[0042] Furthermore, the antioxidant is a compound of a hindered phenol antioxidant and a phosphite antioxidant.

[0043] In this embodiment, the weight ratio of the hindered phenol antioxidant to the phosphite antioxidant in the antioxidant is 1:1. The hindered phenol antioxidant can be Irganox 1010 produced by BASF; and the phosphite antioxidant can be Irganox 168 produced by BASF.

[0044] Furthermore, the stabilizer is at least one of an organic tin heat stabilizer, a lead salt heat stabilizer and a rare earth heat stabilizer.

[0045] In this embodiment, the organic tin heat stabilizer can be selected from the organic tin heat stabilizer with the grade of YT-181 produced by Yunnan Tin Industry; the lead salt heat stabilizer can be selected from the lead salt heat stabilizer with the grade of WWL-202A produced by Weilinna New Materials; and the rare earth heat stabilizer can be selected from the rare earth heat stabilizer with the grade of 102 produced by Linyi Poly New Materials. Preferably, when the stabilizer is a mixture of the organic tin heat stabilizer, the lead salt heat stabilizer and the rare earth heat stabilizer, the weight ratio of the three is 2:1:1.

[0046] In summary, the ABS-PVC alloy material of this embodiment has the following beneficial effects:

[0047] 1) Compared with the existing flame-retardant ABS / PVC materials, the ABS-PVC alloy material of this embodiment reduces the use of flame retardants and reduces the specific gravity (or density) of the ABS-PVC alloy material, thereby saving material costs;

[0048] 2) This embodiment uses a compatible toughening agent and AS resin to promote the compatibility of ABS resin and PVC resin, thereby improving the toughness of the ABS-PVC alloy material, and uses AS resin for volume expansion and reinforcement to ensure the tensile and bending strength of the ABS-PVC alloy material; at the same time, the added AS resin also plays a role in increasing the surface gloss;

[0049] 3) This embodiment uses a glossing agent to further improve the surface gloss of the ABS-PVC alloy material without affecting the mechanical properties and flame retardant properties of the alloy material, thus meeting the requirements of many automotive interior and home appliance exterior parts.

[0050] refer to Figure 1 In another embodiment, the present invention further provides a method for preparing an ABS-PVC alloy material, wherein the ABS-PVC alloy material is the ABS-PVC alloy material in the above embodiment, and the method specifically comprises the following steps:

[0051] Step S10, weighing ABS resin, PVC resin, AS resin, compatible toughening agent, flame retardant, gloss agent, lubricant, antioxidant and stabilizer according to weight parts.

[0052] That is, weigh 50-70 parts of ABS resin, 20-40 parts of PVC resin, 5-10 parts of AS resin, 4-10 parts of compatible toughening agent, 1-5 parts of flame retardant, 0.1-0.4 parts of gloss agent, 0.1-0.5 parts of lubricant, 0.1-0.5 parts of antioxidant and 0.1-0.3 parts of stabilizer respectively.

[0053] Step S20, after drying the ABS resin, the PVC resin and the AS resin, feed them into a high-speed mixer for high-speed stirring to obtain a first mixture; wherein the high-speed stirring is controlled at a speed of 900 to 1000 rpm and a control time of 8 to 12 minutes.

[0054] That is, firstly, preheat the hot air dryer to 80°C, then put the ABS resin, PVC resin and AS resin into the preheated hot air dryer respectively, and keep the drying time for 2 to 4 hours until the water content in the resin reaches the standard requirement, which means that the water content is less than (less than or equal to) 0.05%. Finally, add the dried ABS resin, PVC resin and AS resin into a high-speed mixer, mix and stir at a speed of 900 to 1000 rpm for 8 to 12 minutes, and the first mixture can be obtained.

[0055] Step S30, adding the compatible toughening agent, the flame retardant, the gloss agent, the lubricant, the antioxidant and the stabilizer to the first mixture, stirring at medium to low speed to obtain a second mixture; wherein the controlled speed of the medium to low speed stirring is 400 to 800 rpm, and the controlled time is 4 to 8 minutes.

[0056] That is, the remaining other components are added to the first mixed material obtained in step S20, and the mixture is mixed and stirred at a rotation speed of 400 to 800 rpm for 4 to 8 minutes to obtain the second mixed material.

[0057] Step S40, sending the second mixed material into a twin-screw extruder for extrusion granulation to obtain an ABS-PVC alloy material.

[0058] That is, the second mixed material obtained in step S30 is fed into a twin-screw extruder, and the screw speed is controlled to be 300-500 rpm and the extrusion temperature is controlled to be 190-220° C., and extrusion granulation is performed, and then after drying, an ABS-PVC alloy material is obtained.

[0059] It should be noted that, in other embodiments, ABS resin, PVC resin and AS resin can be weighed first, dried and stirred at high speed to obtain a first mixture; then, a compatible toughening agent, a flame retardant, a gloss agent, a lubricant, an antioxidant and a stabilizer are weighed, added to the first mixture and stirred at medium or low speed to obtain a second mixture; finally, the second mixture is fed into a twin-screw extruder, and after extrusion, cooling, granulation and drying, an ABS-PVC alloy material is obtained.

[0060] The preparation method of the ABS-PVC alloy material is as follows: first, the ABS resin, the PVC resin and the AS resin are dried to ensure that the water content of the resin is reduced to an appropriate level, thereby improving the processing performance of the resin; then, the dried ABS resin, the PVC resin and the AS resin are stirred at a high speed to ensure that the resin is fully and evenly stirred; the remaining other components are further added for medium-low speed stirring to prevent powder from being thrown out and affecting the stirring effect; finally, the stirred mixture is sent to a twin-screw extruder for extrusion granulation to obtain an ABS-PVC alloy material with light material, good toughness, good flame retardant effect and high gloss.

[0061] Below, the present invention will illustrate one or more embodiments through the following examples.These examples are not intended to limit the purpose of the present invention and / or the scope of one or more embodiments.

[0062] Embodiment 1:

[0063] An ABS-PVC alloy material includes the following components in parts by weight: 13 parts of bulk ABS resin, 40 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer. Among them, the compatible toughening agent is chlorinated polyethylene, the flame retardant is a compound of chlorinated polyethylene and antimony trioxide in a weight ratio of 15:1, the glossing agent is a compound of basic heavy metal and amide compound in a weight ratio of 1:1, the lubricant is a pentaerythritol stearate lubricant, the antioxidant is a compound of hindered phenol antioxidant and phosphite antioxidant in a weight ratio of 1:1, and the stabilizer is a compound of organic tin heat stabilizer, lead salt heat stabilizer and rare earth heat stabilizer in a weight ratio of 2:1:1.

[0064] The preparation method of the above-mentioned ABS-PVC alloy material comprises the following steps:

[0065] Step a, respectively weighing 13 parts of bulk ABS resin, 40 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of gloss agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer;

[0066] Step b, after drying the ABS resin, the PVC resin and the AS resin, feeding them into a high-speed mixer, stirring them at a high speed of 900 rpm for 10 minutes, to obtain a first mixed material;

[0067] Step c, adding a compatible toughening agent, a flame retardant, a glossing agent, a lubricant, an antioxidant and a stabilizer to the first mixture, stirring at a medium-low speed of 600 rpm for 6 minutes to obtain a second mixture;

[0068] Step d, feeding the second mixed material into a twin-screw extruder, extruding and granulating at a screw speed of 300 r / min and an extrusion temperature of 200° C., and drying at 90° C. to obtain an ABS-PVC alloy material.

[0069] Embodiment 2:

[0070] An ABS-PVC alloy material comprises the following components in parts by weight: 17 parts of bulk ABS resin, 36 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0071] Embodiment 3:

[0072] An ABS-PVC alloy material comprises the following components in parts by weight: 18 parts of bulk ABS resin, 39 parts of emulsion ABS resin, 30 parts of PVC resin, 4 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0073] Embodiment 4:

[0074] An ABS-PVC alloy material comprises the following components in parts by weight: 18 parts of bulk ABS resin, 47 parts of emulsion ABS resin, 20 parts of PVC resin, 6 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0075] Comparative Example 1:

[0076] An ABS-PVC alloy material comprises the following components in parts by weight: 0 parts of bulk ABS resin, 53 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0077] Comparative Example 2:

[0078] An ABS-PVC alloy material comprises the following components in parts by weight: 53 parts of bulk ABS resin, 0 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0079] Comparative Example 3:

[0080] An ABS-PVC alloy material comprises the following components in parts by weight: 20 parts of bulk ABS resin, 41 parts of emulsion ABS resin, 30 parts of PVC resin, 0 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0081] Comparative Example 4:

[0082] An ABS-PVC alloy material comprises the following components in parts by weight: 17 parts of bulk ABS resin, 36 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 4 parts of compatible toughening agent, 2 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0083] Comparative Example 5:

[0084] An ABS-PVC alloy material comprises the following components in parts by weight: 17 parts of bulk ABS resin, 36 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 8 parts of compatible toughening agent, 0 parts of flame retardant, 0.2 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0085] Comparative Example 6:

[0086] An ABS-PVC alloy material comprises the following components in parts by weight: 13 parts of bulk ABS resin, 40 parts of emulsion ABS resin, 30 parts of PVC resin, 8 parts of AS resin, 6 parts of compatible toughening agent, 2 parts of flame retardant, 0 parts of glossing agent, 0.4 parts of lubricant, 0.2 parts of antioxidant and 0.2 parts of stabilizer.

[0087] The ABS-PVC alloy materials in the above-mentioned Examples 2 to 4 and Comparative Examples 1 to 6 are prepared in a similar manner to that in Example 1. The only difference between them and Example 1 is that the components used are different in content, and the specific component contents are shown in Table 1.

[0088] Table 1 Component weight table of ABS-PVC alloy materials

[0089]

[0090] The following performance tests were performed on the ABS-PVC alloy materials in Examples 1 to 4 and Comparative Examples 1 to 6, and the testing method was as follows: the ABS-PVC alloy material was dried at 90°C, and then injection molded to obtain a standard test specimen, wherein the process conditions for injection molding were as follows: the nozzle temperature was 220°C, the temperatures of the three sections from the feeding section to the nozzle were 205°C, 215°C and 220°C, the holding time was 2 to 4s, and the injection pressure was 40 to 60MPa; further, the tensile strength test was performed with reference to ISO 527:2012 standard; the bending modulus test was performed with reference to ISO 178:2019 standard; the cantilever beam notched impact strength test was performed with reference to ISO 180:2019 standard; the gloss test was performed with reference to ASTM D-523; and the flame retardant performance test of the specimen 1.6mm was performed with reference to UL94, and the test results are shown in Table 2.

[0091] Table 2 Performance test results of ABS-PVC alloy materials

[0092]

[0093] As can be seen from Table 2, the density of the ABS-PVC alloy material in the embodiments and comparative examples of the present invention is between 1.12 and 1.14, while the density of the common ABS-PVC flame retardant material on the market is between 1.16 and 1.19. Therefore, the present invention achieves a reduction in the specific gravity of the alloy material and optimizes the material cost.

[0094] Combining Table 1 and Table 2, it can be seen from Example 2, Comparative Example 4 and Comparative Example 5 that the effect of the compatible toughening agent can improve the overall performance of the alloy material, but adding more compatible toughening agent makes the material softer; it can be seen from Example 2, Example 3, Example 4 and Comparative Example 3 that AS resin plays a role of volume expansion and reinforcement in the ABS-PVC alloy material, and also improves the surface gloss; it can be seen from Comparative Examples 1 and 2 that the surface gloss of the emulsion ABS resin is higher than that of the bulk ABS resin, but the impact strength is lower than that of the bulk ABS resin, so considering the comprehensive performance, the bulk ABS resin and the emulsion ABS resin are used in combination; it can be seen from Example 1 and Comparative Example 6 that adding a small amount of gloss agent can effectively improve the overall gloss of the alloy material without affecting the physical properties and flame retardant properties of the alloy material.

[0095] It can be seen from Example 2, Comparative Example 4 and Comparative Example 5 that polyvinyl chloride can be used as a compatible toughening agent and can also be used synergistically as a flame retardant. When used in combination with antimony trioxide, it can achieve the maximum flame retardant effect and realize V0 flame retardancy.

[0096] It should be noted that, in this article, the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a product or method including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or method. In the absence of more restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the product or method including the element.

[0097] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. An ABS-PVC alloy material, characterized in that: The ABS-PVC alloy material comprises the following components in parts by weight: 50-70 parts of ABS resin, 20-40 parts of PVC resin, 5-10 parts of AS resin, 4-10 parts of compatible toughening agent, 1-5 parts of flame retardant, 0.1-0.4 parts of glossing agent, 0.1-0.5 parts of lubricant, 0.1-0.5 parts of antioxidant and 0.1-0.3 parts of stabilizer.

2. The ABS-PVC alloy material according to claim 1, characterized in that: The ABS resin is a compound of bulk ABS resin and emulsion ABS resin, and the weight ratio of the bulk ABS resin to the emulsion ABS resin is 1:(2-3).

3. The ABS-PVC alloy material according to claim 2, characterized in that: The polymerization degree of the PVC resin is 500.

4. The ABS-PVC alloy material according to claim 3, characterized in that: The compatible toughening agent is at least one of chlorinated polyethylene, ethylene vinyl acetate copolymer, methyl methacrylate-butadiene-styrene copolymer and nitrile rubber.

5. The ABS-PVC alloy material according to claim 4, characterized in that: The flame retardant is a compound of chlorinated polyethylene and antimony trioxide.

6. The ABS-PVC alloy material according to claim 5, characterized in that: The brightener is at least one of a basic heavy metal and an amide compound.

7. The ABS-PVC alloy material according to claim 6, characterized in that: The lubricant is a pentaerythritol stearate lubricant.

8. The ABS-PVC alloy material according to claim 7, characterized in that: The antioxidant is a compound of a hindered phenol antioxidant and a phosphite antioxidant.

9. The ABS-PVC alloy material according to claim 8, characterized in that: The stabilizer is at least one of an organic tin heat stabilizer, a lead salt heat stabilizer and a rare earth heat stabilizer.

10. A method for preparing the ABS-PVC alloy material according to any one of claims 1 to 9, characterized in that: include: Weigh ABS resin, PVC resin, AS resin, compatible toughening agent, flame retardant, gloss agent, lubricant, antioxidant and stabilizer according to weight parts; After drying, the ABS resin, the PVC resin and the AS resin are fed into a high-speed mixer for high-speed stirring to obtain a first mixed material; wherein the high-speed stirring is controlled at a speed of 900 to 1000 rpm and a control time of 8 to 12 minutes; Adding the compatible toughening agent, the flame retardant, the gloss agent, the lubricant, the antioxidant and the stabilizer to the first mixed material, stirring at a medium to low speed to obtain a second mixed material; Wherein, the control speed of the medium-low speed stirring is 400-800rpm, and the control time is 4-8min; The second mixed material is fed into a twin-screw extruder for extrusion granulation to obtain an ABS-PVC alloy material.

Citation Information

Patent Citations

  • High-fluidity PVC / ABS alloy material and preparation method thereof

    CN102453306B