Grafted particle doped sulfonated polyetheretherketone water lubricated bearing material and preparation method thereof
By doping grafted particles into the sulfonated polyether ether ketone material, the problems of insufficient mechanical strength and poor bonding of the water-lubricated bearing material are solved, and the friction and mechanical properties are significantly improved, and the service life is extended.
Patent Information
- Application Number
- CN202411569781.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-06
AI Technical Summary
The lack of mechanical strength of existing water-lubricated bearing materials and poor bonding of lubricating particles with polyether ether ketone materials leads to wear and noise problems.
By ball milling the lubricating particles with the grafting material to form grafting particles, mixed with sulfonated polyether ether ketone powder and carbon fiber, the grafted particles are formed and lubricated with sulfonated polyether ether ketone water lubricating bearing material, strengthening The bonding and mechanical properties of the material.
It improves the friction and mechanical properties of water-lubricated bearing materials, reduces wear rate and friction coefficient, and extends service life.
Smart Images

Figure CN119081347A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material and a preparation method thereof. Background Art
[0002] As a new and environmentally friendly device, water-lubricated bearings have attracted extensive attention from researchers. Its uniqueness lies in its ability to work stably and reliably under water lubrication rather than grease lubrication conditions, and has the characteristics of simple structure, easy processing, no pollution, and long service life. It solves the problems of environmental pollution and resource waste caused by lubricating oil leakage in ship transmission systems from the source, which is conducive to building a new type of ship propulsion system that is pollution-free, widely available, and highly stable. Therefore, water-lubricated bearings have broad application prospects, especially in ship rudder bearings, stern bearings, centrifugal pumps, hydro-turbine generators, water circulation systems and other components.
[0003] When the ship propulsion system is started, the bearing speed is too low and is in a boundary lubrication state, making it difficult to form a complete lubricating water film on its surface. Moreover, under the action of the main shaft and seawater pressure, the bearing load-bearing part is easily deformed, the bearing clearance is reduced, the contact area between the bearing and the sleeve is increased, and the interface roughness peaks are in contact with each other and the interaction force is higher than the material yield stress, which will cause the roughness peaks to deform and break, and eventually cause serious wear of the bearing base material and generate a lot of friction noise, which seriously affects the operation of the ship and greatly shortens the service life of the bearing. Therefore, the preparation technology and evaluation system of high-performance, low-wear, and high-durability water-lubricated bearings urgently need to be established.
[0004] Polyetheretherketone material is a high-performance engineering material. At present, when polyetheretherketone material is directly used as a water-lubricated bearing substrate, due to the large friction coefficient of polyetheretherketone material, it is difficult to form a lubricating water film on the material surface when used as a bearing substrate, which will cause the rough peaks between the interfaces to contact each other, resulting in high wear, high heat generation and high noise, and reducing the service life of the bearing and the spindle. In order to solve the above problems, some researchers have introduced pore structures into sulfonated polyetheretherketone materials by pore-forming sulfonated polyetheretherketone matrix materials. However, the mechanical strength of polyetheretherketone materials with porous structures is insufficient, and the wear degree of polyetheretherketone materials will increase under high load conditions. Some researchers have also enhanced the friction reduction and wear resistance of polyetheretherketone composite materials by doping lubricating particles (solid lubricants) into polyetheretherketone matrix materials. However, the existing lubricating particles have poor bonding with the polyetheretherketone matrix material, and cracks are easily formed at the interface between the lubricating particles and the matrix material during the friction and wear process, which will accelerate the failure and destruction of polyetheretherketone materials.
[0005] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention
[0006] The present invention provides a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material and a preparation method thereof, aiming to solve the problems of insufficient mechanical strength of existing water-lubricated bearing materials and poor bonding between lubricating particles and polyetheretherketone materials: To achieve the above object, the solution provided by the present invention is: A method for preparing a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material comprises the following steps: S001. ball-milling the lubricating particles and the grafting material together to graft the grafting material onto the surface of the lubricating particles to obtain grafted particles, S002. Evenly mix the sulfonated polyetheretherketone powder, carbon fiber and grafted particles, and then put the mixed materials into a mold for cold pressing. S003. After the cold pressing is completed, the formed material is placed in a muffle furnace for sintering to obtain a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material; Wherein, in step S001, the grafting material is at least one of sucrose and urea.
[0007] Optionally, in step S001, the lubricating particles are at least one of molybdenum disulfide and graphite.
[0008] Optionally, in step S001, when the grafting material is sucrose, the mass ratio of the lubricating particles to the grafting material is (0.2-1):1.
[0009] Optionally, in step S001, when the grafting material is urea, the mass ratio of the lubricating particles to the grafting material is 1:(1-1.5).
[0010] Optionally, in step S001, the ball milling speed is 450-550 rpm, and the ball milling time is 10-12 h.
[0011] Optionally, in step S002, the mass ratio of sulfonated polyetheretherketone powder: carbon fiber: grafted particles is (7.6-7.8): (1.0-1.2): (1.0-1.2).
[0012] Optionally, in step S003, the sintering temperature is 360-380°C, and the sintering time is 4-5h.
[0013] Optionally, the pressure of cold pressing is 10 to 120 MPa, and the temperature of cold pressing is 20 to 30°C.
[0014] Optionally, in step S001, after ball milling, the product is soaked in deionized water, and then ultrasonic vibration is performed to disperse the grafted particles in the product. After the ultrasonic vibration is completed, suction filtration is performed to remove unreacted grafted materials in the product from the grafted particles.
[0015] The present invention also provides a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, wherein the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material is prepared by the preparation method of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material.
[0016] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, by doping lubricating particles grafted with sucrose or urea into the polyetheretherketone material, so that hydrophilic groups are introduced into the polyetheretherketone material, thereby not only enabling the polyetheretherketone water-lubricated bearing material to effectively adsorb hydrated cations in seawater to form a more stable hydrated lubricating layer on the surface of the material, but also effectively enhancing the bonding between the grafted particles and the polyetheretherketone matrix material, thereby enhancing the mechanical properties and friction properties of the water-lubricated bearing material, so that the wear rate and friction coefficient of the water-lubricated bearing material can be further reduced compared with the porous sulfonated polyetheretherketone water-lubricated bearing material.
[0017] In addition, the present invention uses sulfonated polyetheretherketone material to dope with grafted particles, and utilizes the hydration effect of the sulfonated group on the sulfonated polyetheretherketone, so that the water-lubricated bearing material can more easily adsorb hydrated cations in seawater, thereby forming a more stable hydrated lubrication layer on the material surface, which can further reduce the friction coefficient and wear degree of the material.
[0018] The present invention also provides a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The provided water-lubricated bearing material can play a supporting role in the friction process, effectively reduce friction and resist wear and extend the service life of the water-lubricated bearing. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention provides a flow chart of the preparation method of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material.
[0020] Figure 2 The friction coefficient curve of the water-lubricated bearing material prepared in Example 1 and Comparative Example 1 is shown.
[0021] Figure 3 The three-dimensional morphology of the wear scar of the water-lubricated bearing material prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, comprising the following steps: S001. The lubricating particles and the grafted material are ball-milled together using a planetary ball mill. The mechanical force generated by the ball milling causes the lubricating particles and the grafted material to collide with each other in a high-energy environment, making it easier for the grafted material to contact and combine with the surface of the lubricating particles. The surface of the lubricating particles can be grafted with the grafted material, thereby obtaining grafted particles. S002. Using an oscillating ball mill, sulfonated polyetheretherketone powder, carbon fiber and grafted particles are mixed evenly, and then the mixed material is placed in a mold for cold pressing. Cold pressing can give the mixed material a greater pressure, increase the density of the material and enhance the mechanical properties and friction properties of the material, so that the surface strength of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material obtained by subsequent sintering is improved. S003. After the cold pressing is completed, the formed material is placed in a muffle furnace for sintering to obtain the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material. The sintering process ensures the melting of the sulfonated polyetheretherketone powder and is more tightly combined with the carbon fiber and the grafted particles, thereby enhancing the mechanical properties and friction properties of the water-lubricated bearing material.
[0024] In step S001 of the above preparation method, the lubricating particles can be used as filler particles in the polyetheretherketone matrix material and the water-lubricated bearing material. When the lubricating particles are nanometer-sized, the lubricating particles have excellent surface effect and quantum size effect, which can enhance the friction performance of the water-lubricated bearing material, so that the wear rate and friction coefficient of the material can be effectively reduced.
[0025] The grafted material is at least one of sucrose and urea. Sucrose has multiple hydroxyl functional groups, and urea has multiple amino functional groups. Both hydroxyl functional groups and amino functional groups are hydrophilic groups. When the grafted material is grafted on the surface of the lubricating particles, the amino functional groups and hydroxyl functional groups can effectively absorb hydrated cations in seawater to form a hydrated lubricating layer on the surface of the material, thereby achieving a lubricating effect.
[0026] In step S002 of the above preparation method, the sulfonated polyetheretherketone powder is obtained by sulfonation modification of polyetheretherketone material. Compared with the polyetheretherketone material that has not been sulfonated, the sulfonated polyetheretherketone material is more hydrophilic. In addition, because the surface of the lubricating particles is grafted with a grafted material with a hydroxyl functional group or an amino functional group, the water-lubricated bearing material can more easily adsorb hydrated cations in seawater, thereby forming a more stable hydrated lubricating layer on the surface of the material.
[0027] Moreover, since the hydroxyl functional group and the amino functional group are easily combined with the polyetheretherketone material, the lubricating particles grafted with sucrose or urea have a stronger bonding ability with the sulfonated polyetheretherketone matrix material, which can overcome the problem of poor bonding between the existing solid lubricants and the matrix. When the lubricating particles are doped into the sulfonated polyetheretherketone material, the water-lubricated bearing material can have the improvement in mechanical properties and friction properties that the lubricating particles can bring.
[0028] In step S002 of the above preparation method, the carbon fiber has high strength and modulus. By doping the carbon fiber into the sulfonated polyetheretherketone powder, the compressive strength of the water-lubricated bearing material can be significantly improved, so that the material has better resistance under low-speed and heavy-load conditions.
[0029] It can be seen that the present invention introduces hydrophilic groups into the sulfonated polyetheretherketone material by doping lubricating particles grafted with sucrose or urea, thereby enabling the sulfonated polyetheretherketone water-lubricated bearing material to effectively adsorb hydrated cations in seawater to form a more stable hydrated lubricating layer on the surface of the material, and also enhancing the bonding between the grafted particles and the polyetheretherketone matrix material, thereby enhancing the mechanical properties and friction properties of the water-lubricated bearing material, and enabling the wear rate and friction coefficient of the water-lubricated bearing material to be further reduced compared with the porous sulfonated polyetheretherketone water-lubricated bearing material.
[0030] Optionally, in step S001, the lubricating particles are at least one of molybdenum disulfide and graphite. Compared with traditional lubricating particles such as silicon nitride, molybdenum disulfide and graphite are more easily combined with the polyetheretherketone matrix material after graft modification. During the friction and wear process, cracks are not easily formed at the interface between the lubricating particles and the matrix, and the failure and damage of the water-lubricated bearing material will not be accelerated.
[0031] Optionally, in step S001, when the grafting material is sucrose, the mass ratio of the lubricating particles to the grafting material is (0.2-1): 1. The above mass ratio is a preferred mass ratio of the lubricating particles to the grafting material, which can not only make the lubricating particles fully grafted and modified by the grafting material, but also the yield of the grafted particles will not be too low.
[0032] When the grafted material is urea, the preferred mass ratio of the lubricating particles to the grafted material is 1:(1-1.5).
[0033] Optionally, in step S001 of the preparation method, the ball milling speed is 450-550 rpm, and the ball milling time is 10-12 hours. When the ball milling speed and the ball milling time are controlled within the above parameter range, it can ensure that the grafted material is fully grafted onto the surface of the lubricating particles, the content of unreacted grafted material in the grafted product is small, and the yield of the grafted particles is high.
[0034] Optionally, in step S002, the mass ratio of sulfonated polyetheretherketone powder: carbon fiber: grafted particles is (7.6-7.8): (1.0-1.2): (1.0-1.2). When the mass ratio of sulfonated polyetheretherketone powder: carbon fiber: grafted particles is controlled within the above range, the friction performance and mechanical properties of the water-lubricated bearing material can be maintained at a better level at the same time, and the water-lubricated bearing material has both a low friction coefficient and high compression strength.
[0035] Optionally, in step S003 of the above preparation method, the sintering temperature is 360-380°C and the sintering time is 4-5h. When the sintering temperature and sintering time are controlled within the above parameter range, the sulfonated polyetheretherketone powder can be fully melted and more closely combined with the carbon fiber and the grafted particles, so that the mechanical properties and friction properties of the water-lubricated bearing material are enhanced.
[0036] Optionally, the pressure of cold pressing is 10-120 MPa, and the temperature of cold pressing is 20-30° C. By controlling the pressure and temperature of cold pressing within the above parameter range, the sulfonated polyetheretherketone powder, carbon fiber and grafted particles can be more closely combined, and the strength of the surface of the water-lubricated bearing material can be enhanced.
[0037] Optionally, in step S001 of the preparation method, after ball milling, the product is soaked in deionized water, and then ultrasonically oscillated for more than 2 hours to disperse the grafted particles in the product. After the ultrasonic oscillation, the product is filtered using a filter membrane. The soaking-dispersion-filtration process can be repeated multiple times until the unreacted grafted material in the product is completely removed from the grafted particles.
[0038] After the unreacted grafted material is completely removed from the grafted particles, no holes will be generated in the sulfonated polyetheretherketone material due to the decomposition of urea and sucrose, and the mechanical strength of the sulfonated polyetheretherketone material will not be insufficient. Therefore, under high load, the wear degree of the water-lubricated bearing material will not increase.
[0039] After the unreacted grafted material in the product is completely removed from the grafted particles, the filtered grafted particles are dried in an oven at a drying temperature of 75 to 85° C. to completely remove the moisture in the grafted particles. After the moisture in the grafted particles is completely removed, it is beneficial to control the ratio of various materials in the water-lubricated bearing material before cold pressing the water-lubricated bearing material, so that the mechanical properties and friction properties of the sintered water-lubricated bearing material can be enhanced.
[0040] Optionally, in step S002, the sulfonated polyetheretherketone powder is prepared by the following preparation method, specifically, comprising the following steps: H001. Dry the polyetheretherketone powder in a blast drying oven; H002. Add an organic solvent into a three-necked flask, then add the dried polyetheretherketone powder into the three-necked flask, then drop a sulfonating agent into the three-necked flask, stir mechanically, and react at room temperature for 2.5 to 3.5 hours to allow the polyetheretherketone to react with the sulfonating agent to generate sulfonated polyetheretherketone; H003. The reaction product of step H002 is poured into a container filled with ice water, and then the pH of the reaction product is adjusted to neutral with a pH adjuster; H004. Wash and filter the reaction product with a neutral pH value with deionized water to obtain sulfonated polyetheretherketone powder.
[0041] In the above step H001, the drying temperature is 120° C. and the drying time is 8 hours to remove moisture from the polyetheretherketone powder, thereby avoiding serious agglomeration of polyetheretherketone particles and the reaction between water vapor and solvent, which is unfavorable to the sulfonation modification of polyetheretherketone.
[0042] In the above step H003, the reaction product is poured into a container filled with ice water to prevent the pH adjuster from releasing heat violently when adjusting the pH of the reaction product. The pH adjuster may be sodium hydroxide.
[0043] Optionally, in step H002, the organic solvent is dichloromethane and tetrahydrofuran. As organic solvents, dichloromethane and tetrahydrofuran can disperse the polyetheretherketone particles and avoid serious agglomeration of the polyetheretherketone particles, thereby facilitating the regulation of the sulfonation degree of the polyetheretherketone, so that the polyetheretherketone material after sulfonation modification has higher surface hardness and better friction performance; in addition, dichloromethane and tetrahydrofuran are safer and easier to scale up the test than other organic solvents, so they can be used for batch modification of polyetheretherketone powder, providing a guarantee for the application of polyetheretherketone materials to large components such as water-lubricated bearings.
[0044] Optionally, in step H002, the sulfonating agent is at least one of chlorosulfonic acid and aminosulfonic acid. Compared with other types of sulfonating agents, the sulfonation reaction of chlorosulfonic acid, aminosulfonic acid and polyetheretherketone is controllable. When polyetheretherketone reacts with the sulfonating agent, no obvious agglomeration phenomenon will occur in the organic solvent, and no large amount of heat will be released, which has high safety. This helps to regulate the sulfonation degree of the polyetheretherketone material, so that the sulfonated modified material can have both high surface hardness and good friction properties, thereby providing a guarantee for the application of polyetheretherketone materials in large components such as water-lubricated bearings.
[0045] Optionally, in step H002, the mass ratio of the organic solvent to the polyetheretherketone powder is 100:(1-5). At this mass ratio, the polyetheretherketone powder can be effectively dispersed in the organic solvent, so that the polyetheretherketone powder is sulfonated and modified.
[0046] Optionally, in step H002, the volume ratio of dichloromethane to tetrahydrofuran is 4:1, and the dispersibility of the polyetheretherketone powder in the organic solvent can be significantly improved, so that the polyetheretherketone powder is well sulfonated and modified.
[0047] Optionally, in step H002, the mass ratio of the organic solvent to the sulfonating agent is 100:(1-4). When the mass ratio of the sulfonating agent to the organic solvent is within the above range, the sulfonation effect of the polyetheretherketone powder is better, so that the sulfonated modified polyetheretherketone powder has excellent hydration effect characteristics.
[0048] The present invention also provides a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, wherein the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material is prepared by the above-mentioned preparation method of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The provided water-lubricated bearing material can play a supporting role in the friction process, effectively reduce friction and resist wear, and extend the service life of the water-lubricated bearing.
[0049] In order to further illustrate the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material provided by the present invention, the following examples and comparative examples are provided.
[0050] Example 1 This embodiment provides a method for preparing a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material, comprising the following steps: S001. Use a planetary ball mill to ball-mill the molybdenum disulfide lubricating particles and sucrose (grafted material) together. The mass ratio of molybdenum disulfide to sucrose is 1: (1-1.5). The rotation speed of the planetary ball mill is 500 rpm. The ball milling time is 12 hours, so that sucrose is grafted on the surface of the molybdenum disulfide. After the reaction is completed, the product is soaked in deionized water and then ultrasonically oscillated for 2 hours to disperse the grafted modified molybdenum disulfide particles in the product. After the ultrasonic oscillation is completed, the product is filtered using a filter membrane. The above soaking-dispersion-filtration process is repeated many times until the unreacted sucrose in the product is completely removed from the grafted modified molybdenum disulfide particles, and then the grafted modified molybdenum disulfide particles are dried in an oven at 80°C for standby use.
[0051] S002. 3.8 g of sulfonated polyetheretherketone powder, 0.6 g of carbon fiber and 0.6 g of grafted modified molybdenum disulfide particles were mixed evenly by an oscillating ball mill, and then the mixed material was placed in a mold with a diameter of 20 mm and cold pressed at a pressure of 10 MPa; S003. After the cold pressing is completed, the formed material is placed in a muffle furnace for sintering at 360° C. for 2 hours to obtain a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material.
[0052] Example 2 This embodiment provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: (1) In step S001, the lubricating particles are graphite; (2) In step S002, the mass of sulfonated polyetheretherketone powder is 4.0 g, the mass of carbon fiber is 0.6 g, and the mass of grafted modified graphite is 0.4 g.
[0053] Example 3 This embodiment provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S002, the mass of sulfonated polyetheretherketone powder is 4.2 g, the mass of carbon fiber is 0.6 g, and the mass of grafted modified molybdenum disulfide is 0.2 g.
[0054] Example 4 This embodiment provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S001, the grafting material is urea, and the mass ratio of molybdenum disulfide to urea is 1:1.5.
[0055] Comparative Example 1 This comparative example provides a method for preparing a lubricating particle-doped sulfonated polyetheretherketone water-lubricated bearing material, comprising the following steps: S001. 3.8 g of sulfonated polyetheretherketone powder, 0.6 g of carbon fiber and 0.6 g of ungrafted molybdenum disulfide particles were mixed evenly by an oscillating ball mill, and then the mixed material was placed in a mold with a diameter of 20 mm and cold pressed at a pressure of 10 MPa; S002. After the cold pressing is completed, the formed material is placed in a muffle furnace for sintering at 360° C. for 2 hours to obtain a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material.
[0056] Comparative Example 2 This comparative example provides a method for preparing a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those in Example 1, including steps S001, S002, and S003, but there are the following differences: In step S001, the mass ratio of molybdenum disulfide to sucrose is 1:0.7.
[0057] Comparative Example 3 This comparative example provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S001, the grafting material is urea, and the mass ratio of molybdenum disulfide to urea is 1:0.7.
[0058] Comparative Example 4 This comparative example provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S002, the mass of sulfonated polyetheretherketone powder is 3.8 g, the mass of carbon fiber is 0 g, and the mass of grafted modified molybdenum disulfide is 1.2 g.
[0059] Comparative Example 5 This comparative example provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S002, the mass of the sulfonated polyetheretherketone powder is 3.8 g, the mass of the carbon fiber is 1.0 g, and the mass of the grafted modified molybdenum disulfide is 0.2 g.
[0060] Comparative Example 6 This comparative example provides a method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material. The steps of the preparation method are basically the same as those of Example 1, including steps S001, S002, and S003, but there are the following differences: In step S002, the mass of sulfonated polyetheretherketone powder is 4.4 g, the mass of carbon fiber is 0.0 g, and the mass of grafted modified molybdenum disulfide is 0.6 g.
[0061] The friction performance of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Examples 1 to 4, the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Example 1, and the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Examples 2 to 6 were tested using a UMT rotary friction and wear tester. The test conditions were: speed 100-600rpm, load 15N, gyration radius 5mm, and 3% sodium chloride solution was selected as the test environment. The test results are as follows: Figure 2 And as shown in Table 1.
[0062] Among them, Table 1 shows the friction coefficient values of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Examples 1 to 4, the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Example 1, and the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Examples 2 to 6 when the test machine speed is 600 rpm.
[0063] Figure 2 The friction curves of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1 and the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 1 are shown. Figure 2It can be seen that when the speed of the test machine is 100rpm, after testing for 1800s, the friction coefficient of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1 is 0.024, while the friction coefficient of the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 1 is 0.031. When the speed of the test machine is increased to 600rpm, after testing for 1800s, the friction coefficient of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1 is 0.009, reaching a super-slip state, while the friction coefficient of the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 1 is 0.020. Therefore, by comparison, it can be seen that the friction performance of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1 is significantly better than that of the lubricating particles doped with sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 1.
[0064] This is because, when preparing the water-lubricated bearing material, the comparative example 1 did not dope the grafted modified lubricating particles into the sulfonated polyetheretherketone material, while when preparing the water-lubricated bearing material, the example 1 doped the grafted modified lubricating particles into the sulfonated polyetheretherketone material, thereby not only introducing the sulfonated group into the material, but also introducing the hydrophilic groups such as hydroxyl and amino groups, improving the compatibility and binding of the lubricating particles with the sulfonated polyetheretherketone material, and further improving the hydrophilicity of the polyetheretherketone material. The presence of the sulfonate group and the grafted hydrophilic group on the surface of the polyetheretherketone enhances the adsorption of hydrated sodium ions at the material interface, and the formed hydration layer has the characteristics of reducing friction and anti-wear, and the modified lubricating particles are more likely to form a solid lubricating film, reducing the shear stress between the surface of the sulfonated polyetheretherketone material and the friction pair surface, thereby effectively reducing the friction and wear of the interface.
[0065] The three-dimensional morphology of the wear scar of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1 and the lubricating particle-doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 1 after the friction performance test was completed was observed by using a three-dimensional white light interferometer. The three-dimensional morphology of the wear scar is shown in FIG. Figure 3 ,from Figure 3 It can be seen that after the friction performance test of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1, the wear depth on the material surface is reduced, and the furrows inside the wear marks are reduced. It can be seen that the friction reduction and wear resistance of the material are improved, indicating that the introduction of sulfonic acid groups and hydrophilic groups into the polyetheretherketone material can effectively improve the hydrophilicity of the polyetheretherketone material, promote the formation of a lubricating water film on the material surface and reduce the friction coefficient and wear degree.
[0066] Table 1 Friction coefficient at 600rpm Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 0.009 0.016 0.025 0.012 0.015 0.020 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 0.021 0.025 0.031 0.025
[0067] It can be seen from the test results in Table 1 that the friction coefficient of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Examples 2 and 3 gradually increases compared with the friction coefficient of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Example 1. This is because the amount of grafted particles doped into the sulfonated polyetheretherketone material is gradually reduced when preparing the water-lubricated bearing material in Examples 2 and 3. When the amount of grafted particles doped into the sulfonated polyetheretherketone material is reduced, the friction performance of the material is improved, but the degree of improvement is limited.
[0068] It can be seen from the test results in Table 1 that the friction coefficient of the grafted particles doped with sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Examples 2 and 3 is higher than that in Comparative Example 1. This is because in Comparative Examples 2 and 3, when the lubricating particles are grafted with the grafted material, the amount of grafted material used is relatively small, so that the lubricating particles cannot be fully grafted and modified, and there is still a problem of poor bonding between the lubricating particles and the sulfonated polyetheretherketone material. The strength of the material surface cannot be effectively provided and it is easy to wear.
[0069] The compression strength test of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material samples prepared in Example 1 and Comparative Examples 2 to 6 with a diameter of 20 mm and a height of 10 mm was performed using a universal testing machine. The test results are shown in Table 2: Table 2: Compression strength(MPa) Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 180 173 165 102 183 113 It can be seen from the test results in Table 2 that the compressive strength of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Examples 4 and 6 is not as good as the compressive strength of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing materials prepared in Example 1. This is because the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing materials prepared in Comparative Examples 4 and 6 are not doped with carbon fibers, and carbon fibers have the effect of improving the compressive strength of water-lubricated bearing materials, making the materials have better resistance under low-speed and heavy-load conditions, and can simultaneously maintain the friction properties and mechanical properties of the water-lubricated bearing materials at an optimal level. The water-lubricated bearing material has both a low friction coefficient and high compressive strength.
[0070] It can be seen from the test results in Table 2 that although the compressive strength of the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 5 is relatively high, its friction coefficient value is also relatively large, and the friction performance cannot be enhanced. This is because the amount of carbon fiber doping in the grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material prepared in Comparative Example 5 is too much, while the amount of grafted particle doping is too little, and the water-lubricated bearing material cannot simultaneously have excellent friction performance and mechanical properties.
[0071] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, characterized in that: The following steps are involved: S001. ball-milling the lubricating particles and the grafting material together to graft the grafting material onto the surface of the lubricating particles to obtain grafted particles, S002. Evenly mix the sulfonated polyetheretherketone powder, carbon fiber and grafted particles, and then put the mixed materials into a mold for cold pressing. S003. After the cold pressing is completed, the formed material is placed in a muffle furnace for sintering to obtain a grafted particle-doped sulfonated polyetheretherketone water-lubricated bearing material; Wherein, in step S001, the grafting material is at least one of sucrose and urea.
2. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S001, the lubricating particles are at least one of molybdenum disulfide and graphite.
3. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S001, when the grafting material is sucrose, the mass ratio of the lubricating particles to the grafting material is (0.2-1):
1.
4. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S001, when the grafting material is urea, the mass ratio of the lubricating particles to the grafting material is 1:(1-1.5).
5. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S001, the ball milling speed is 450-550 rpm, and the ball milling time is 10-12 h.
6. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S002, the mass ratio of sulfonated polyetheretherketone powder: carbon fiber: grafted particles is (7.6-7.8): (1.0-1.2): (1.0-1.2).
7. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S003, the sintering temperature is 360-380°C, and the sintering time is 4-5h.
8. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: The pressure of cold pressing is 10 to 120 MPa, and the temperature of cold pressing is 20 to 30°C.
9. The method for preparing the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to claim 1, characterized in that: In step S001, after the ball milling is completed, the product is soaked in deionized water, and then ultrasonic vibration is performed to disperse the grafted particles in the product. After the ultrasonic vibration is completed, suction filtration is performed to remove the unreacted grafted materials in the product from the grafted particles.
10. A grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material, characterized in that: The grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material is prepared by the preparation method of the grafted particle doped sulfonated polyetheretherketone water-lubricated bearing material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Polyarylether / nano expanded graphite / carbon fiber high-strength conducting composite material and preparation method thereof
CN101875774A
High-performance airplane empennage composite material and its preparation technology
CN102875966A
Metal lining plastic anti-corrosion and rub-resistant composite as well as preparation method and application thereof
CN106751443A
Preparation method of conductive polyether ether ketone composite material
CN108102292A
Porous sulfonated polyetheretherketone water-lubricated bearing material and preparation method thereof
CN117327238A
Cited By
Method for preparing anti-oxidation molybdenum coating on surface of polyether-ether-ketone base material
CN120514924A