High-toughness heat-conducting PC composite material and preparation method thereof
By adding modified polyurethane elastomer and thermal filler to PC materials, a thermal conductivity network is formed, which solves the problems of insufficient high toughness, thermal conductivity and flame retardant performance of PC materials, and achieves the improvement of high toughness, thermal conductivity and flame retardant performance. .
Patent Information
- Application Number
- CN202411347402.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-26
AI Technical Summary
PC materials have problems such as poor notch sensitivity, insufficient thermal conductivity and flame retardant properties in applications of high toughness materials, which limits their use in practical applications.
Using the preparation method of high-tough thermal conductivity PC composite material, by adding modified polyurethane elastomer and thermal filler to the PC resin, silicon carbide is modified with γ-aminopropyltriethoxysilane to form amino-amino-carbide and carbide by carbide Silicon @COF and maleic anhydride are coated with polypropylene to form a thermal conductivity network to improve the thermal conductivity and flame retardant properties of the material.
It significantly improves the toughness, thermal conductivity and flame retardant properties of the material, forms an excellent thermal conductivity network, enhances mechanical properties, avoids stress concentration and crack propagation, and meets the needs of high toughness, thermal conductivity and flame retardant properties.
Smart Images

Figure BDA0005061352550000101 
Figure BDA0005061352550000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer composite materials, and in particular to a high-toughness thermally conductive PC composite material and a preparation method thereof. Background Art
[0002] Polycarbonate (PC) material is one of the five most widely used engineering plastics. With its unique characteristics of high light transmittance, high refractive index, high impact resistance, dimensional stability and easy processing and molding, it is widely used in various industries such as optical materials, electronic appliances, automobile manufacturing, packaging and building materials. However, PC material still has some disadvantages and needs to be modified.
[0003] During the processing of PC materials, its unique segment structure and degree of entanglement determine its excellent comprehensive performance. However, due to the high crack initiation energy and low crack propagation energy of polycarbonate, its notch sensitivity is poor and it is prone to stress cracking, which limits its application in high-toughness materials. Its performance needs to be further improved. In addition, although PC materials have certain thermal conductivity and flame retardancy, with the increase in practical application requirements, the thermal conductivity and flame retardancy of PC materials themselves no longer meet the requirements. Therefore, researchers need to develop a PC composite material with high toughness, good thermal conductivity and good flame retardancy to meet actual needs. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a high-toughness thermally conductive PC composite material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A high-toughness thermally conductive PC composite material, comprising the following raw materials in parts by weight: 70-90 parts of PC resin, 8-12 parts of modified polyurethane elastomer, 5-10 parts of thermally conductive filler, 0.1-0.5 parts of antioxidant, and 0.2-0.5 parts of lubricant;
[0007] The thermally conductive filler is prepared by the following steps:
[0008] Step A1, dispersing γ-aminopropyltriethoxysilane in ethanol, heating to 60°C and stirring for 30 minutes, then heating to 70-80°C, adding silicon carbide and deionized water, stirring for 3-5 hours, centrifuging, washing, and drying to obtain amino silicon carbide;
[0009] Step A2, 2,5-diaminophenol hydrochloride and triethylamine are uniformly dispersed in N,N-dimethylformamide, and then cyanuric chloride and amino silicon carbide are added and ultrasonically treated for 30 minutes, and then transferred to an autoclave, reacted at 120-140° C. for 8-12 hours, and then centrifuged, washed, and dried to obtain silicon carbide @COF;
[0010] Step A3, adding maleic anhydride grafted polypropylene and silicon carbide @COF into acetone and dispersing them evenly, slowly dropping 4-dimethylaminopyridine acetone solution, and then sequentially adding triethylamine, 2-chloro-1-methylpyridinium iodide and dichloromethane, and reacting under nitrogen for 12-18 hours, rotary evaporation, washing, and freeze drying to obtain a thermal conductive filler;
[0011] Further, in step A1, the usage ratio of γ-aminopropyltriethoxysilane, ethanol, silicon carbide and deionized water is 1-2 mL: 100 mL: 3-6 g: 10 mL;
[0012] Further, in step A2, the usage ratio of 2,5-diaminophenol hydrochloride, triethylamine, N,N-dimethylformamide, cyanuric chloride and amino silicon carbide is 0.1-0.2 mol: 15 mL: 200 mL: 0.05-0.1 mol: 0.5-1.2 g;
[0013] Furthermore, in step A3, the amount ratio of maleic anhydride grafted polypropylene, silicon carbide @COF, acetone, 4-dimethylaminopyridine acetone solution, triethylamine, 2-chloro-1-methylpyridinium iodide and dichloromethane is 0.05-0.2 mol: 1-3 g: 200 mL: 30 mL: 0.05-0.15 mol: 0.001-0.003 mol: 20 mL, and the 4-dimethylaminopyridine acetone solution is prepared by mixing 4-dimethylaminopyridine and acetone in a dosage ratio of 0.001-0.002 mol: 30 mL.
[0014] The modified polyurethane elastomer is prepared by the following steps:
[0015] Step B1, under nitrogen conditions, allylamine and 3,5-dihydroxybenzoic acid are mixed evenly, and heated to 180-200 ° C for reaction for 3-5h, and then heated to 220 ° C for reaction for 2-3h, and then the temperature is lowered to room temperature, the intermediate product is collected, and 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxa and azobisisobutyronitrile are added to the intermediate product and stirred evenly, and then the temperature is raised to 70-80 ° C for reaction for 8-12h, and filtered to obtain a phosphorus-containing product;
[0016] Step B2, dispersing the phosphorus-containing product in acetonitrile, adding β-alanine and mixing evenly, heating to 65-75° C. and reflux reaction for 18-24 hours, rotary evaporation and drying to obtain an amino-terminated chain extender;
[0017] Step B3, polyethylene glycol (M n=1000) vacuum dehydration at 120-140°C for 1-3h, argon gas is introduced, and then the temperature is lowered to 70-90°C, isophorone diisocyanate and dibutyltin dilaurate are added to react for 2-4h, and then toluene and terminal amino chain extender are added and stirred for reaction for 2-3h to obtain a modified polyurethane elastomer;
[0018] Further, in step B1, the usage ratio of allylamine, 3,5-dihydroxybenzoic acid, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and azobisisobutyronitrile is 0.01-0.02 mol: 0.015-0.03 mol: 0.01-0.02 mol: 0.08-0.16 g;
[0019] Further, in step B2, the ratio of the phosphorus-containing product, acetonitrile and β-alanine is 0.01-0.03 mol: 200 mL: 0.012-0.035 mol;
[0020] Furthermore, in step B3, the usage ratio of polyethylene glycol, isophorone diisocyanate, dibutyltin dilaurate, toluene and amino-terminated chain extender is 0.1 mol: 0.15-0.25 mol: 0.001-0.005 mol: 30-50 mL: 0.01-0.03 mol.
[0021] A method for preparing a high-toughness thermally conductive PC composite material comprises the following steps:
[0022] Step S1, weighing raw materials by weight, adding PC resin, modified polyurethane elastomer, thermal conductive filler, antioxidant and lubricant into a high-speed mixer, mixing for 5-10 minutes at 60-100° C. and 800-1200 rpm to obtain a mixture;
[0023] Step S2, transferring the mixed material to a twin-screw extruder, extruding and granulating, and obtaining a high-toughness thermally conductive PC composite material;
[0024] Furthermore, the temperature of each section in the twin-screw extruder is: section 1: 220-240°C, section 2 230-250°C, section 3: 240-250°C, section 4 255-265°C, section 5: 260-270°C, section 6: 270-280°C, the head temperature is 270-290°C, and the screw speed is 100-300rpm / min.
[0025] Beneficial effects of the present invention:
[0026] The PC composite material of the present invention is based on PC resin as the matrix, and modified polyurethane elastomer is added to improve the mechanical properties of the matrix and give the matrix higher toughness; thermal conductive filler is added to form a thermal conductive network in the matrix, so that the matrix has excellent thermal conductivity; in addition, the toughness and flame retardant properties of the matrix are also improved through the synergistic effect between the two.
[0027] In the thermal conductive filler, the surface of silicon carbide is first modified with γ-aminopropyltriethoxysilane to synthesize amino silicon carbide; then the amino group on the surface of silicon carbide reacts with the -Cl group in COF to form silicon carbide@COF containing hydroxyl groups; finally, silicon carbide@COF is coated with maleic anhydride grafted polypropylene to synthesize thermal conductive filler. The introduction of thermal conductive filler can improve the thermal conductivity, flame retardancy and mechanical properties of the matrix; among them, silicon carbide and COF can produce a synergistic effect to form a thermal conductive network in the matrix and thus improve the thermal conductivity of the matrix. This is because silicon carbide itself has excellent thermal conductivity, and then it is coated with COF on the surface. The periodic layered structure and pore structure of COF further improve the thermal conductivity of silicon carbide, and the silicon carbide@COF modified with maleic anhydride grafted polypropylene has excellent dispersibility in the matrix, thereby further improving the thermal conductivity of the matrix. High; the maleic anhydride group in the filler can undergo an esterification reaction with the terminal hydroxyl group generated after PC is heated, thereby forming a chemical bond, and the polypropylene chain segment on the surface of the filler will be entangled with the modified polyurethane elastomer molecular chain. Therefore, the filler can improve the interface compatibility between PC and polyurethane molecular chains through esterification reaction and molecular chain entanglement, which in turn helps to transfer stress on the interface, avoid stress concentration, inhibit crack propagation, and improve the mechanical properties of the matrix; in addition, silicon carbide, COF and polypropylene can also work synergistically to give the matrix certain flame retardant properties.
[0028] In the modified polyurethane elastomer, an amide reaction between an amino group in allylamine and a hydroxyl group in 3,5-dihydroxybenzoic acid is firstly used to synthesize an intermediate product, and then a double bond structure in the intermediate product is used to react with active hydrogen in 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxa to synthesize a phosphorus-containing product; then an esterification reaction is carried out between the hydroxyl group in the phosphorus-containing product and the carboxyl group in beta-alanine to obtain an amino-terminated chain extender; finally, polyethylene glycol, isophorone diisocyanate and an amino-terminated chain extender are used as raw materials, and dibutyltin dilaurate is used as a catalyst to synthesize the modified polyurethane elastomer. The addition of modified polyurethane elastomer can utilize its own excellent toughness to improve the toughness of the matrix, and at the same time can also improve the flame retardant performance of the matrix; among them, the amino chain extender introduced into the modified polyurethane elastomer can give the matrix better toughness than the traditional hydroxyl chain extender, because the amino chain extender can extend the molecular chain in the polyurethane molecular chain and increase the molecular weight, thereby significantly improving the mechanical properties of the polyurethane elastomer; the 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxa introduced into the amino chain extender gives the polyurethane elastomer excellent flame retardant performance, and can cooperate with the thermal conductive filler to flame retardant, so that the matrix has certain flame retardant performance. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] The thermal conductive filler is prepared by the following steps:
[0032] Step A1, disperse 1 mL of γ-aminopropyltriethoxysilane in 100 mL of ethanol, heat to 60° C. and stir for 30 min, then heat to 70° C., add 3 g of silicon carbide and 10 mL of deionized water, stir and react for 3 h, centrifuge, wash and dry to obtain amino silicon carbide;
[0033] Step A2, 0.1 mol of 2,5-diaminophenol hydrochloride and 15 mL of triethylamine were evenly dispersed in 200 mL of N,N-dimethylformamide, and then 0.05 mol of cyanuric chloride and 0.5 g of amino silicon carbide were added and ultrasonically treated for 30 min, and then transferred to an autoclave, reacted at 120° C. for 8 h, and then centrifuged, washed, and dried to obtain silicon carbide @COF;
[0034] Step A3, 0.05 mol maleic anhydride grafted polypropylene and 1 g silicon carbide @COF are added to 200 mL acetone and dispersed evenly, 30 mL 4-dimethylaminopyridine acetone solution is slowly added dropwise, and then 0.05 mol triethylamine, 0.001 mol 2-chloro-1-methylpyridinium iodide and 20 mL dichloromethane are added in sequence, and reacted for 12 hours under nitrogen conditions, rotary evaporated, washed, and freeze-dried to obtain a thermal conductive filler. The 4-dimethylaminopyridine acetone solution is prepared by mixing 4-dimethylaminopyridine and acetone in a dosage ratio of 0.001 mol:30 mL.
[0035] The modified polyurethane elastomer is prepared by the following steps:
[0036] Step B1, under nitrogen conditions, 0.01 mol of allylamine and 0.015 mol of 3,5-dihydroxybenzoic acid were mixed evenly, heated to 180 ° C for reaction for 3 h, heated to 220 ° C for reaction for 2 h, and then the temperature was lowered to room temperature, the intermediate product was collected, and 0.01 mol of 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and 0.08 g of azobisisobutyronitrile were added to the intermediate product and stirred evenly, and then heated to 70 ° C for reaction for 8 h, and filtered to obtain a phosphorus-containing product;
[0037] Step B2, dispersing 0.01 mol of the phosphorus-containing product in 200 mL of acetonitrile, adding 0.012 mol of β-alanine and mixing evenly, heating to 65° C. and reflux reaction for 18 h, rotary evaporation and drying to obtain an amino-terminated chain extender;
[0038] Step B3, 0.1 mol polyethylene glycol (M n =1000) was vacuum dehydrated at 120°C for 1h, argon was introduced, and then the temperature was lowered to 70°C, 0.15mol of isophorone diisocyanate and 0.001mol of dibutyltin dilaurate were added and reacted for 2h, and then 30mL of toluene and 0.01mol of terminal amino chain extender were added and stirred for reaction for 2h to obtain a modified polyurethane elastomer.
[0039] Example 2
[0040] The thermal conductive filler is prepared by the following steps:
[0041] Step A1, disperse 1.5 mL of γ-aminopropyltriethoxysilane in 100 mL of ethanol, heat to 60° C. and stir for 30 min, then heat to 75° C., add 4.5 g of silicon carbide and 10 mL of deionized water, stir and react for 4 h, centrifuge, wash and dry to obtain amino silicon carbide;
[0042] Step A2, 0.15 mol of 2,5-diaminophenol hydrochloride and 15 mL of triethylamine were evenly dispersed in 200 mL of N,N-dimethylformamide, and then 0.075 mol of cyanuric chloride and 0.8 g of amino silicon carbide were added and ultrasonically treated for 30 min, and then transferred to an autoclave, reacted at 130° C. for 10 h, and then centrifuged, washed, and dried to obtain silicon carbide @COF;
[0043] Step A3, 0.1 mol maleic anhydride grafted polypropylene and 2 g silicon carbide @COF are added to 200 mL acetone and dispersed evenly, 30 mL 4-dimethylaminopyridine acetone solution is slowly added dropwise, and then 0.1 mol triethylamine, 0.002 mol 2-chloro-1-methylpyridinium iodide and 20 mL dichloromethane are added in sequence, and reacted under nitrogen for 15 hours, rotary evaporated, washed, and freeze-dried to obtain a thermal conductive filler. The 4-dimethylaminopyridine acetone solution is prepared by mixing 4-dimethylaminopyridine and acetone in a dosage ratio of 0.0015 mol:30 mL.
[0044] The modified polyurethane elastomer is prepared by the following steps:
[0045] Step B1, under nitrogen conditions, 0.015 mol of allylamine and 0.02 mol of 3,5-dihydroxybenzoic acid were mixed evenly, heated to 190 ° C for reaction for 4 hours, heated to 220 ° C for reaction for 2.5 hours, and then the temperature was lowered to room temperature, the intermediate product was collected, and then 0.015 mol of 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and 0.12 g of azobisisobutyronitrile were added to the intermediate product and stirred evenly, and then heated to 75 ° C for reaction for 10 hours, and filtered to obtain a phosphorus-containing product;
[0046] Step B2, dispersing 0.02 mol of the phosphorus-containing product in 200 mL of acetonitrile, adding 0.022 mol of β-alanine and mixing evenly, heating to 70° C. and reflux reaction for 22 h, rotary evaporation and drying to obtain an amino-terminated chain extender;
[0047] Step B3, 0.1 mol polyethylene glycol (M n =1000) was vacuum dehydrated at 130°C for 2h, argon was introduced, and then the temperature was lowered to 80°C, 0.2mol of isophorone diisocyanate and 0.003mol of dibutyltin dilaurate were added and reacted for 3h, and then 40mL of toluene and 0.02mol of terminal amino chain extender were added and stirred for reaction for 2.5h to obtain a modified polyurethane elastomer.
[0048] Example 3
[0049] The thermal conductive filler is prepared by the following steps:
[0050] Step A1, disperse 2 mL of γ-aminopropyltriethoxysilane in 100 mL of ethanol, heat to 60° C. and stir for 30 min, then heat to 80° C., add 6 g of silicon carbide and 10 mL of deionized water, stir and react for 5 h, centrifuge, wash and dry to obtain amino silicon carbide;
[0051] Step A2, 0.2 mol of 2,5-diaminophenol hydrochloride and 15 mL of triethylamine were evenly dispersed in 200 mL of N,N-dimethylformamide, and then 0.1 mol of cyanuric chloride and 1.2 g of amino silicon carbide were added and ultrasonically treated for 30 min, and then transferred to an autoclave, reacted at 140° C. for 12 h, and then centrifuged, washed, and dried to obtain silicon carbide @COF;
[0052] Step A3, 0.2 mol maleic anhydride grafted polypropylene and 3 g silicon carbide @COF are added to 200 mL acetone and dispersed evenly, 30 mL 4-dimethylaminopyridine acetone solution is slowly added dropwise, and then 0.15 mol triethylamine, 0.003 mol 2-chloro-1-methylpyridinium iodide and 20 mL dichloromethane are added in sequence, and reacted under nitrogen for 18 hours, rotary evaporated, washed, and freeze-dried to obtain a thermal conductive filler. The 4-dimethylaminopyridine acetone solution is prepared by mixing 4-dimethylaminopyridine and acetone in a dosage ratio of 0.002 mol:30 mL.
[0053] The modified polyurethane elastomer is prepared by the following steps:
[0054] Step B1, under nitrogen conditions, 0.02 mol of allylamine and 0.03 mol of 3,5-dihydroxybenzoic acid were mixed evenly, heated to 200 ° C for reaction for 5 h, heated to 220 ° C for reaction for 3 h, then lowered to room temperature, the intermediate product was collected, and 0.02 mol of 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and 0.16 g of azobisisobutyronitrile were added to the intermediate product and stirred evenly, then heated to 80 ° C for reaction for 12 h, filtered to obtain a phosphorus-containing product;
[0055] Step B2, dispersing 0.03 mol of the phosphorus-containing product in 200 mL of acetonitrile, adding 0.035 mol of β-alanine and mixing evenly, heating to 75° C. and reflux reaction for 24 h, rotary evaporation and drying to obtain an amino-terminated chain extender;
[0056] Step B3, 0.1 mol polyethylene glycol (M n =1000) was vacuum dehydrated at 140°C for 3h, argon was introduced, and then the temperature was lowered to 90°C, 0.25mol of isophorone diisocyanate and 0.005mol of dibutyltin dilaurate were added and reacted for 4h, and then 50mL of toluene and 0.03mol of terminal amino chain extender were added and stirred for reaction for 3h to obtain a modified polyurethane elastomer.
[0057] Example 4
[0058] A method for preparing a high-toughness thermally conductive PC composite material comprises the following steps:
[0059] 70 parts of PC resin, 8 parts of the modified polyurethane elastomer prepared in Example 1, 5 parts of the thermal conductive filler prepared in Example 1, 0.1 parts of antioxidant H161, and 0.2 parts of zinc stearate;
[0060] Step S1, weighing raw materials by weight, adding PC resin, modified polyurethane elastomer prepared in Example 1, thermal conductive filler prepared in Example 1, antioxidant H161 and zinc stearate into a high-speed mixer, and mixing for 5 minutes at 60° C. and 800 rpm to obtain a mixture;
[0061] Step S2, transferring the mixed material to a twin-screw extruder, extruding and granulating, and obtaining a high-toughness thermal conductive PC composite material. The temperatures of each section in the twin-screw extruder are: section 1: 220°C, section 2: 230°C, section 3: 240°C, section 4: 255°C, section 5: 260°C, section 6: 270°C, the die head temperature is 270°C, and the screw speed is 100rpm / min.
[0062] Example 5
[0063] A method for preparing a high-toughness thermally conductive PC composite material comprises the following steps:
[0064] 80 parts of PC resin, 10 parts of the modified polyurethane elastomer prepared in Example 2, 7 parts of the thermal conductive filler prepared in Example 2, 0.3 parts of antioxidant H161, and 0.4 parts of zinc stearate;
[0065] Step S1, weighing raw materials by weight, adding PC resin, modified polyurethane elastomer prepared in Example 2, thermal conductive filler prepared in Example 2, antioxidant H161 and zinc stearate into a high-speed mixer, and mixing for 8 minutes at 80° C. and 1000 rpm to obtain a mixture;
[0066] Step S2, transferring the mixed material to a twin-screw extruder, extruding and granulating, and obtaining a high-toughness thermal conductive PC composite material. The temperatures of each section in the twin-screw extruder are: section 1: 230°C, section 2: 240°C, section 3: 245°C, section 4: 260°C, section 5: 265°C, section 6: 275°C, the head temperature is 280°C, and the screw speed is 200rpm / min.
[0067] Example 6
[0068] A method for preparing a high-toughness thermally conductive PC composite material comprises the following steps:
[0069] 90 parts of PC resin, 12 parts of the modified polyurethane elastomer prepared in Example 3, 10 parts of the thermal conductive filler prepared in Example 3, 0.5 parts of antioxidant H161, and 0.5 parts of zinc stearate;
[0070] Step S1, weighing raw materials by weight, adding PC resin, modified polyurethane elastomer prepared in Example 3, thermal conductive filler prepared in Example 3, antioxidant H161 and zinc stearate into a high-speed mixer, and mixing for 10 minutes at 100° C. and 200 rpm to obtain a mixture;
[0071] Step S2, transferring the mixed material to a twin-screw extruder, extruding and granulating, and obtaining a high-toughness thermal conductive PC composite material. The temperatures of each section in the twin-screw extruder are: section 1: 240°C, section 2: 250°C, section 3: 250°C, section 4: 265°C, section 5: 270°C, section 6: 280°C, the die head temperature is 290°C, and the screw speed is 300rpm / min.
[0072] Comparative Example 1
[0073] This comparative example is a PC composite material, which differs from Example 6 in that silicon carbide is used instead of the thermal conductive filler prepared in Example 3, and the rest are the same.
[0074] Comparative Example 2
[0075] This comparative example is a PC composite material, which is different from Example 6 in that a commercially available polyurethane elastomer is used instead of the modified polyurethane elastomer prepared in Example 3, and the rest are the same.
[0076] The PC composite materials in Examples 4-6 and Comparative Examples 1-2 were injection molded according to ISO standards, and the injection molded specimens were stabilized at 23° C. and 50% relative humidity for 48 hours before performance testing:
[0077] The test results are shown in the following table:
[0078]
[0079]
[0080] As can be seen from the above table, after the mechanical properties, thermal conductivity and flame retardancy tests of the PC composite material prepared by the present invention, the tensile strength is in the range of 68.61MPa-74.56MPa, the notched impact strength is in the range of 56.4J / m-59.1J / m, and the thermal conductivity is 5.6W / m -1 K -1 -59.1W / m -1 K -1 The flame retardant grade is VTM-0, indicating that the composite material has excellent toughness, thermal conductivity and flame retardant properties.
[0081] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A high-toughness thermally conductive PC composite material, It is characterized in that The invention comprises the following raw materials in parts by weight: 70-90 parts of PC resin, 8-12 parts of modified polyurethane elastomer, 5-10 parts of thermal conductive filler, 0.1-0.5 parts of antioxidant, and 0.2-0.5 parts of lubricant; The thermally conductive filler is prepared by the following steps: Step A1, dispersing γ-aminopropyltriethoxysilane in ethanol, heating to 60°C and stirring for 30 minutes, then heating to 70-80°C, adding silicon carbide and deionized water, stirring for 3-5 hours, centrifuging, washing, and drying to obtain amino silicon carbide; Step A2, 2,5-diaminophenol hydrochloride and triethylamine are uniformly dispersed in N,N-dimethylformamide, and then cyanuric chloride and amino silicon carbide are added and ultrasonically treated for 30 minutes, and then transferred to an autoclave, reacted at 120-140° C. for 8-12 hours, and then centrifuged, washed, and dried to obtain silicon carbide @COF; Step A3, add maleic anhydride grafted polypropylene and silicon carbide @COF into acetone and disperse them evenly, slowly drop 4-dimethylaminopyridine acetone solution, then add triethylamine, 2-chloro-1-methylpyridinium iodide and dichloromethane in sequence, and react under nitrogen for 12-18h, rotary evaporate, wash, and freeze-dry to obtain a thermal conductive filler.
2. A high-toughness thermally conductive PC composite material according to claim 1, It is characterized in that In step A1, the usage ratio of γ-aminopropyltriethoxysilane, ethanol, silicon carbide and deionized water is 1-2 mL: 100 mL: 3-6 g: 10 mL.
3. The high-toughness thermally conductive PC composite material according to claim 1, It is characterized in that In step A2, the usage ratio of 2,5-diaminophenol hydrochloride, triethylamine, N,N-dimethylformamide, cyanuric chloride and amino silicon carbide is 0.1-0.2 mol:15 mL:200 mL:0.05-0.1 mol:0.5-1.2 g.
4. The high-toughness thermally conductive PC composite material according to claim 1, It is characterized in that In step A3, the amount ratio of maleic anhydride grafted polypropylene, silicon carbide @COF, acetone, 4-dimethylaminopyridine acetone solution, triethylamine, 2-chloro-1-methylpyridinium iodide and dichloromethane is 0.05-0.2 mol: 1-3 g: 200 mL: 30 mL: 0.05-0.15 mol: 0.001-0.003 mol: 20 mL, and the 4-dimethylaminopyridine acetone solution is prepared by mixing 4-dimethylaminopyridine and acetone in a dosage ratio of 0.001-0.002 mol: 30 mL.
5. The high-toughness thermally conductive PC composite material according to claim 1, It is characterized in that The modified polyurethane elastomer is prepared by the following steps: Step B1, under nitrogen conditions, allylamine and 3,5-dihydroxybenzoic acid are mixed evenly, and heated to 180-200 ° C for reaction for 3-5h, and then heated to 220 ° C for reaction for 2-3h, and then the temperature is lowered to room temperature, the intermediate product is collected, and 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxa and azobisisobutyronitrile are added to the intermediate product and stirred evenly, and then the temperature is raised to 70-80 ° C for reaction for 8-12h, and filtered to obtain a phosphorus-containing product; Step B2, dispersing the phosphorus-containing product in acetonitrile, adding β-alanine and mixing evenly, heating to 65-75° C. and reflux reaction for 18-24 hours, rotary evaporation and drying to obtain an amino-terminated chain extender; Step B3, dehydrate polyethylene glycol in vacuo at 120-140°C for 1-3h, introduce argon, then cool to 70-90°C, add isophorone diisocyanate and dibutyltin dilaurate to react for 2-4h, then add toluene and amino-terminated chain extender and stir to react for 2-3h to obtain modified polyurethane elastomer.
6. The high-toughness thermally conductive PC composite material according to claim 5, It is characterized in that In step B1, the usage ratio of allylamine, 3,5-dihydroxybenzoic acid, 9,10-dihydro-9-oxa-10-phosphophanol-10-oxa and azobisisobutyronitrile is 0.01-0.02 mol: 0.015-0.03 mol: 0.01-0.02 mol: 0.08-0.16 g.
7. The high-toughness thermally conductive PC composite material according to claim 5, It is characterized in that The usage ratio of the phosphorus-containing product, acetonitrile and β-alanine in step B2 is 0.01-0.03 mol:200 mL:0.012-0.035 mol.
8. The high-toughness thermally conductive PC composite material according to claim 5, It is characterized in that In step B3, the usage ratio of polyethylene glycol, isophorone diisocyanate, dibutyltin dilaurate, toluene and amino-terminated chain extender is 0.1 mol: 0.15-0.25 mol: 0.001-0.005 mol: 30-50 mL: 0.01-0.03 mol.
9. A method for preparing the high-toughness thermally conductive PC composite material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Step S1, weighing raw materials by weight, adding PC resin, modified polyurethane elastomer, thermal conductive filler, antioxidant and lubricant into a high-speed mixer, mixing for 5-10 minutes at 60-100° C. and 800-1200 rpm to obtain a mixture; Step S2: transferring the mixed material to a twin-screw extruder, extruding and granulating, and obtaining a high-toughness thermally conductive PC composite material.
10. A method for preparing a high-toughness thermally conductive PC composite material according to claim 9, It is characterized in that The temperature of each section in the twin-screw extruder is: section 1: 220-240°C, section 2 230-250°C, section 3: 240-250°C, section 4 255-265°C, section 5: 260-270°C, section 6: 270-280°C, the head temperature is 270-290°C, and the screw speed is 100-300rpm / min.
Citation Information
Patent Citations
Corrosion-resistant and high-temperature-resistant composite plastic and production process thereof
CN111978639A
Heat-conducting flame-retardant PC composite material and preparation method thereof
CN114806130A
Polyurethane composite material for runway and preparation method thereof
CN115322558A
Metal ceramic composite coating material for non-stick pan and preparation method of metal ceramic composite coating material
CN117327429A