Nylon composite material and preparation method thereof
By integrating halloysite nanotubes and glass fibers with flame retardants in a twin-screw extrusion process, the nylon composite material addresses hydrolysis and oxidative aging issues, achieving enhanced durability and mechanical properties.
Patent Information
- Application Number
- CN202411569775.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nylon 66 composites face issues with rapid hydrolysis under humid conditions, oxidative aging due to glass fiber reinforcement, and precipitation of flame retardants in high temperature and humidity environments, which degrade mechanical properties and limit durability.
A nylon composite material is prepared by mixing halloysite nanotubes and glass fibers with APTES, forming a composite powder with a flame retardant, and then melt-extruding with nylon and other additives to enhance interfacial bonding and inhibit flame retardant precipitation, using a twin-screw extruder.
The resulting composite material exhibits improved resistance to moisture and heat aging, with enhanced mechanical properties and prolonged flame retardant stability, demonstrating superior performance in mechanical tests.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a nylon composite material and a preparation method thereof. Background Art
[0002] Polyamide 66 (PA66) degrades rapidly under humid conditions due to the hydrolysis of amide bonds, which greatly reduces the mechanical properties of the material and limits its durability. Glass fiber reinforced nylon composites, because the addition of glass fiber will catalyze the oxidative aging and hydrolytic degradation of nylon, the main failure mode is interface debonding. Flame retardant reinforced PA66 composites, in the halogen-free flame retardant nylon system, the traditional flame retardant is mainly a compound of diethylphosphinate and melamine polyphosphate. The flame retardant is easy to precipitate in a high temperature and high humidity environment, forming needle-shaped or block-shaped grains. Summary of the invention
[0003] In view of the fact that the main challenges in developing a flame-retardant reinforced nylon 66 composite material that is resistant to moisture and heat aging are the need to reduce the hydrolysis of the nylon matrix, increase the interfacial bonding of the glass fiber, and limit the precipitation of the flame retardant, the present invention provides a nylon composite material and a preparation method thereof, so that the nylon composite material has excellent flame retardancy.
[0004] To achieve the above object, the embodiments of the present invention adopt the following technical solutions: A method for preparing a nylon composite material comprises the following steps: S1: Mix halloysite nanotubes (HNT) and glass fibers with toluene, add a certain amount of APTES to react, reflux the mixture under stirring, and dry the solid in the mixture to obtain functionalized HNT and glass fibers; S2: premixing the modified HNT, glass fiber and flame retardant by rotation to obtain a composite powder; S3: The composite powder, nylon, long carbon chain nylon, toughening agent, coupling agent, antioxidant and lubricant are added into a twin-screw extruder for melt co-extrusion to obtain a nylon composite material.
[0005] Preferably, the weight parts of each raw material in the step are: 35-65 parts of nylon, 5-15 parts of long carbon chain nylon, 15-35 parts of glass fiber, 1-5 parts of HNT, 2-10 parts of flame retardant, 0.1-1 parts of toughening agent, 1-7 parts of coupling agent, 0.01-5 parts of antioxidant, and 0.01-5 parts of lubricant.
[0006] Preferably, in step S1, the solute to solution ratio of the HNT and glass fiber to toluene is 1 g:100 mL.
[0007] Preferably, in step S1, the suspension is refluxed for 6-8 hours and heating is stopped for 14-16 hours.
[0008] Preferably, in step S1, the recovered powder is washed by mixing with toluene after centrifugation.
[0009] Preferably, in step S1, 40-60 ml of toluene is added each time when mixing with toluene, and the process is repeated 4-6 times.
[0010] Preferably, in step S1, the drying temperature is 80-100° C., and the drying time is 24 hours.
[0011] Preferably, in step S2, the premixing time is 3-8 min, the processing temperature is 170-190° C., and the rotor speed is 50-70 rpm.
[0012] Preferably, in step S3, the temperature of zone 1 of the twin-screw extruder is 215-235°C, the temperature of zone 2 is 240-260°C, the temperature of zone 3 is 240-260°C, the temperature of zone 4 is 240-260°C, the temperature of zone 5 is 235-255°C, the temperature of zone 6 is 235-255°C, the temperature of zone 7 is 225-245°C, the temperature of zone 8 is 210-230°C, the temperature of zone 9 is 210-230°C, the temperature of zone 10 is 210-230°C, the temperature of zone 11 is 235-255°C, the screw speed of the extruder is 300-500 rpm, and the residence time is 2-4min.
[0013] On the other hand, a nylon composite material is prepared by the above-mentioned preparation method and is mainly used in the production of automobile interior and exterior decoration, communication equipment, electronic appliances, etc.
[0014] The advantages of the implementation of the present invention are as follows: by adding long carbon chain nylon, flame retardant, APTS modified glass fiber and modified HNT four phases into PA66, by reducing the amide bond density, enhancing the interface interaction force, limiting the movement of nylon molecular chains, inhibiting the precipitation of flame retardant, and finally through twin-screw reactive extrusion, a flame retardant reinforced nylon 66 composite material resistant to moisture and heat aging is developed. DETAILED DESCRIPTION
[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Unless otherwise specified, the raw materials used are all commercially available conventional products, and the nylon material used is nylon 66.
[0017] Example 1
[0018] A nylon composite material is prepared by the following preparation method: S1: A certain amount of HNT and glass fiber were suspended in toluene (the ratio of solute to solution was 1 g: 100 mL). Then a certain amount of APTES was added and the suspension was refluxed for 7 hours under stirring. The heating was stopped for 15 hours, and the recovered solid was washed with toluene by centrifugation and re-suspension cycle, using 40 ml of toluene each time and repeated 5 times. Then the solid in the mixed solution was dried in an oven at 90 ° C for 24 hours to obtain modified HNT and modified glass fiber.
[0019] S2: premixing the modified HNT, modified glass fiber and flame retardant for 5 min using a torque rheometer, with a processing temperature of 180 °C and a rotor speed of 60 rpm to obtain a composite powder; S3: Add composite powder, nylon, long carbon chain nylon, toughening agent, coupling agent, antioxidant and lubricant into a twin-screw extruder for melt co-extrusion, extruder temperature: zone 1 temperature is 215-235°C, zone 2 temperature is 240-260°C, zone 3 temperature is 240-260°C, zone 4 temperature is 240-260°C, zone 5 temperature is 235-255°C, zone 6 temperature is 235-255°C, zone 7 temperature is 225-245°C, zone 8 temperature is 210-230°C, zone 9 temperature is 210-230°C, zone 10 temperature is 210-230°C, zone 11 temperature is 235-255°C, extruder screw speed is 300-500 rpm, residence time is 2-4min. After screw extrusion, cooling, drying and pelletizing are performed to obtain a nylon composite material.
[0020] Examples 1-4 are nylon composite materials of the present invention. The raw materials and weight proportions of the nylon composite materials of Examples 1-4 are shown in Table 1.
[0021] Table 1: Raw materials and weight parts of nylon composite materials in the examples
[0022] The preparation methods of the nylon composite materials of Examples 2-3 are the same as that of Example 1, except that the weight proportions of nylon and long carbon chain nylon are different, as shown in Table 1.
[0023] The preparation method of the nylon composite material of Example 4 is consistent with that of Example 1, except that the weight proportions of nylon and HNT are different, as shown in Table 1.
[0024] The preparation methods of the nylon composite materials of Comparative Examples 1 to 5 are consistent with that of Example 1. The raw materials and weight portions of the nylon composite materials of Comparative Examples 1 to 5 are shown in Table 2.
[0025] Table 2: Raw materials and weight proportions of nylon composite materials in comparative example
[0026] The preparation method of the nylon composite material in Comparative Example 1 is consistent with that in Example 1, except that no long carbon chain nylon, HNT and coupling agent are added.
[0027] The preparation method of the nylon composite material in Comparative Example 2 is consistent with that in Example 1, except that HNT and coupling agent are not added.
[0028] The preparation method of the nylon composite material of Comparative Example 3 is consistent with that of Example 1, and the difference from Example 1 is that no long carbon chain nylon and coupling agent are added.
[0029] The preparation method of the nylon composite material of Comparative Example 4 is consistent with that of Example 1, and the difference from Example 1 is that long carbon chain nylon and HNT are not added.
[0030] The preparation method of the nylon composite material of Comparative Example 5 is consistent with that of Example 1, and the difference from Example 1 is that long carbon chain nylon is not added.
[0031] Test Case Used to test the fracture resistance, tensile properties and impact resistance of the nylon composite materials prepared in various embodiments and comparative examples.
[0032] The elongation at break (%) was tested in accordance with GB / T 1040-2018 standard at a speed of 50 mm / min. Five specimens were tested for each sample and the results were taken as the average value.
[0033] Tensile strength (MPa): The test was carried out in accordance with GB / T 1040-2018 standard, with a speed of 50 mm / min. Five specimens were tested for each sample, and the results were taken as the average value.
[0034] The flexural modulus (MPa) was tested according to GB / T 9341-2008 standard at a speed of 2 mm / min. Five specimens were tested for each sample and the results were averaged.
[0035] Bending strength (MPa): Tested in accordance with GB / T 9341-2008 standard, with a speed of 2mm / min. Five specimens were tested for each sample and the results were averaged.
[0036] Notched impact strength (KJ / m2): Tested in accordance with GB / T 1043.1-2008 standard, the pendulum energy is 2J, 10 specimens are tested for each sample, and the results are taken as the average value.
[0037] UL 94 (0.8 mm): Tested according to ASTM D 618, the sample thickness is 0.8 mm. After the flame is removed after ignition, the sample can quickly self-extinguish and no burning melt drips within 10 seconds.
[0038] Double 85: Carried out under the conditions of 85°C temperature and 85% relative humidity.
[0039] The test results are shown in Table 3.
[0040] Table 3: Test results of nylon composite materials of examples and comparative examples
[0041] It can be seen from Table 3 that when the technical solution of the present invention is adopted, the obtained nylon composite material can inhibit the precipitation of the flame retardant and has excellent mechanical properties; the comprehensive mechanical properties exceed the nylon composite materials described in Comparative Examples 1 to 5; the flame retardant precipitation time is longer and can reach 6 weeks or more, among which the nylon composite materials described in Examples 1 and 2 have the best comprehensive performance.
[0042] Since no long carbon chain nylon was added to Comparative Example 5, the elongation at break and the notched impact strength of the final nylon composite material were lower than those of Examples 1-4, and the flame retardant precipitation time was shorter than that of Examples 1-4; since no HNT and long carbon chain nylon were added to Comparative Example 4, the mechanical properties of the final product were affected; since no long carbon chain nylon and coupling agent were added to Comparative Example 3, the elongation at break and the notched impact strength were lower than those of Examples 1-4, and since no HNT and coupling agent were added to Comparative Example 2, its mechanical properties were also greatly affected; since no long carbon chain nylon, HNT and coupling agent were added to Comparative Example 1, the mechanical properties of the obtained product and the effect of inhibiting the precipitation of flame retardants were poor compared with Examples 1-4.
[0043] The advantages of the implementation of the present invention are as follows: by adding long carbon chain nylon, flame retardant, APTS modified glass fiber and modified HNT four phases into PA66, by reducing the amide bond density, enhancing the interface interaction force, limiting the movement of nylon molecular chains, inhibiting the precipitation of flame retardant, and finally through twin-screw reactive extrusion, a flame retardant reinforced nylon 66 composite material resistant to moisture and heat aging is developed.
[0044] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for preparing a nylon composite material, characterized in that: The following steps are involved: S1: mixing halloysite nanotubes and glass fibers with toluene, adding a preset amount of APTES for reaction, refluxing the mixture under stirring, and drying the solid in the mixture to obtain modified halloysite nanotubes and modified glass fibers; S2: premixing the modified halloysite nanotubes, the modified glass fibers and the flame retardant by rotation to obtain a composite powder; S3: The composite powder, nylon, long carbon chain nylon, toughening agent, coupling agent, antioxidant and lubricant are added into a twin-screw extruder for melt co-extrusion to obtain a nylon composite material.
2. The method for preparing the nylon composite material according to claim 1, characterized in that: The weight parts of the raw materials in the steps are: 35-65 parts of nylon, 5-15 parts of long carbon chain nylon, 15-35 parts of glass fiber, 1-5 parts of halloysite nanotubes, 2-10 parts of flame retardant, 0.1-1 parts of toughening agent, 1-7 parts of coupling agent, 0.01-5 parts of antioxidant, and 0.01-5 parts of lubricant.
3. The method for preparing the nylon composite material according to claim 1, characterized in that: In the step S1, the solute to solution ratio of the halloysite nanotubes and glass fibers to toluene is 1 g:100 mL.
4. The method for preparing the nylon composite material according to claim 1, characterized in that: In step S1, the suspension is refluxed for 6-8 hours, and heating is stopped for 14-16 hours.
5. The method for preparing the nylon composite material according to claim 1, characterized in that: In the step S1, the recovered powder is washed by mixing with toluene after centrifugation.
6. The method for preparing the nylon composite material according to claim 5, characterized in that: In the step S1, 40-60 ml of toluene is added each time when mixing with toluene, and the process is repeated 4-6 times.
7. The method for preparing a nylon composite material according to claim 1, characterized in that: In the step S1, the drying temperature is 80-100° C. and the drying time is 24 hours.
8. The method for preparing a nylon composite material according to claim 1, characterized in that: In the step S2, the premixing time is 3-8 minutes, the processing temperature is 170-190° C., and the rotor speed is 50-70 rpm.
9. The method for preparing a nylon composite material according to claim 1, characterized in that: In the step S3, the temperature of zone 1 of the twin-screw extruder is 215-235°C, the temperature of zone 2 is 240-260°C, the temperature of zone 3 is 240-260°C, the temperature of zone 4 is 240-260°C, the temperature of zone 5 is 235-255°C, the temperature of zone 6 is 235-255°C, the temperature of zone 7 is 225-245°C, the temperature of zone 8 is 210-230°C, the temperature of zone 9 is 210-230°C, the temperature of zone 10 is 210-230°C, the temperature of zone 11 is 235-255°C, the screw speed of the extruder is 300-500 rpm, and the residence time is 2-4 min.
10. A nylon composite material, characterized in that: The nylon composite material is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for wear-resistant high-strength nylon composite material
CN102627854A
Wear-resistant high-strength nylon composite material
CN102634202A
High CTI (Comparative Tracking Index) flame retardant glass fiber reinforced PA6 (Polyamide 6) / PA610 (Polyamide 610) alloy composite
CN102732001A
Halogen-free flame-retarding nylon composite material
CN102850787A
PA66 composite material composition with favorable appearance and high static pressure resistance and preparation method of PA66 composite material composition