Material of degradable biomass-based straw and preparation process

By using biomass materials such as rice husk powder and shell powder, combined with specific additives and preparation processes, a degradable straw with good mechanical properties and hydrophobic properties is prepared, which solves the problems of high cost, difficulty in degradation and easy deformation of the straw material, and realizes the problem of achieving high temperature and high temperature, Environmentally friendly and efficient straw solutions.

CN119081436APending Publication Date: 2024-12-06XIAMEN INCREDIBLE HUSK BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410596668.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing straw materials are costly, difficult to degrade, insufficient mechanical properties, easy to deform and mold, resulting in poor environmental pollution and poor user experience, limiting the large-scale production and application of biomass straws.

Method used

Rice husk powder and shell powder are used as the main raw materials, combined with polyhydroxy fatty acid esters, chitin, tannin, cetyl trimethoxysilane and dopamine, to improve mechanical and hydrophobic properties through the preparation process, and to be frozen by vacuum Dry and UV ultraviolet ozone sterilization treatment to prepare a biomass-based pipette.

Benefits of technology

It realizes low-cost and environmentally friendly recycling of biological waste, extends the service life and storage time of straws, improves mechanical and antibacterial properties, solves the problem of straws becoming soft in water, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081436A_ABST
    Figure CN119081436A_ABST
Patent Text Reader

Abstract

The invention provides a material of a degradable biomass-based straw. The material of the degradable biomass-based straw is prepared from the following components in parts by weight: 50 to 100 parts of rice hull powder, 20 to 70 parts of shell powder, 20 to 60 parts of polyhydroxyalkanoate, 10 to 30 parts of chitin, 5 to 30 parts of tannic acid, 5 to 20 parts of hexadecyltrimethoxysilane and 2 to 10 parts of dopamine. The invention further provides a preparation process of the degradable biomass-based straw. The preparation process is used for preparing the degradable biomass-based straw. The degradable biomass-based straw obtained by the invention has good degradability, mechanical toughness, oxidation resistance and antibacterial property, is simple in production process, high in production efficiency, wide in raw material source, low in cost, green and environment-friendly, has no pressure on the environment, is suitable for wide popularization and application, can replace a disposable plastic straw, and has wide application prospects. The problems that a disposable plastic straw in the prior art is difficult to degrade, high in cost and prone to causing environmental and marine ecological pollution are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable materials, in particular to a material and a preparation process of a degradable biomass-based straw. Background Art

[0002] Plastic packaging accounts for 30% of global consumption, and the use of reusable materials to disposable materials is growing at an increasingly rapid rate. Currently, more than 99% of plastic packaging, including disposable straws, plastic bags and tableware, is made of petroleum-based polymers. These plastic packaging usually exist in the environment for hundreds of years, not only causing serious environmental pollution, but also posing a great threat to human health. With the introduction of plastic purchase restrictions and the development of green chemistry in the world, the development of new degradable materials using renewable biomass resources has received widespread attention.

[0003] At present, the straws on the market include paper straws, PLA straws, bagasse straws, stainless steel straws, glass straws, silicone straws and bamboo straws, which greatly reduce the use of disposable plastic products in daily life. However, there are many problems in the production process of the above-mentioned straws: either the cost of the raw materials used is high, the production process is cumbersome, and it puts great financial and storage pressure on the company, such as glass straws and silicone straws; or the mechanical strength is insufficient and the service life is short, such as paper straws and PLA straws; or the degradability is not high, and there is secondary pollution to the environment, such as bagasse straws; or the obtained straws are easily softened and scattered when exposed to water during use, such as paper straws; or they are not easy to clean, easy to mold, and the user experience is poor, such as bamboo straws and stainless steel straws. The above problems greatly limit the large-scale production and application of biomass straws.

[0004] Rice husk is the main byproduct of rice processing. Generally, 200 kg of rice husk is produced from processing 1 ton of rice. It is one of the most common agricultural product processing wastes in China. China produces more than 200 million tons of rice annually, and more than 40 million tons of rice husk waste resources are generated. Rice husk contains cellulose, hemicellulose, lignin, silicon compounds, crude protein and crude fat, etc. It is an important biomass resource with great utilization value. At present, rice husk is mainly used as fuel or directly treated as waste. The comprehensive utilization rate is insufficient and it is far from being fully utilized.

[0005] In view of this, the inventors specially designed a material and preparation process for a degradable biomass-based straw. This case was thus generated. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a biodegradable biomass-based straw material and preparation process, which is intended to solve the problems of existing straws being difficult to degrade, high in cost, and prone to causing environmental pollution and marine ecological pollution; specifically, using discarded biomass resources such as rice husks and shells as the main raw materials, it greatly reduces production costs and is environmentally friendly; at the same time, hydrophobic agents and antibacterial agents are added to improve the mechanical properties, hydrophobicity and antibacterial properties of biomass straws; and the biodegradable biomass-based straw material has a long service life, is not easy to deform, and has broad application prospects. The technical solution of the present invention is as follows:

[0007] A biodegradable biomass-based straw material, comprising the following components in parts by weight:

[0008] 50-100 parts of rice husk powder;

[0009] 20-70 parts of shell powder;

[0010] Polyhydroxyalkanoate (PHA) 20-60 parts;

[0011] Chitosan 10-30 parts;

[0012] Tannic acid 5-30 parts;

[0013] Hexadecyltrimethoxysilane (HDTMS) 5-20 parts;

[0014] Dopamine 2-10 parts.

[0015] Furthermore, the preparation process of the chitosan is as follows:

[0016] (1) Add the cleaned carapace into a hydrochloric acid solution and stir vigorously at a certain temperature for 3-8 hours;

[0017] (2) then treated with sodium hydroxide to remove strongly bound proteins;

[0018] (3) centrifugation, washing, and dialyzing the suspension until the pH is neutral;

[0019] (4) Freeze-drying the suspension in a vacuum freeze dryer to obtain chitosan.

[0020] Furthermore, the shell is the shell of a marine arthropod, an insect, etc., and the mass of the shell is 1-20g and the temperature is 60-120 degrees; wherein the marine arthropod is any one or any two or more of shrimp, crab, mantis shrimp, and lobster.

[0021] Furthermore, the concentrations of the hydrochloric acid and sodium hydroxide are 1-10 mol / L and 2-8 mol / L, respectively.

[0022] Furthermore, the temperature of the vacuum freeze dryer is minus 50-80°C, and the freezing time is 12-24 hours.

[0023] Furthermore, the rice husk powder is agricultural waste generated in the rice production process, and its average particle size is 100-2000 meshes.

[0024] Furthermore, the average particle size of the shell powder is 200 to 5000 meshes.

[0025] The present invention also provides a preparation process of a degradable biomass-based straw, comprising the following steps:

[0026] (1) weighing rice husk powder, shell powder, chitosan, tannic acid, hexadecyltrimethoxysilane and dopamine in proportion, adding them into a high-speed mixer, mixing and stirring, then adding a certain amount of polyhydroxyalkanoate, and continuing to stir;

[0027] (2) When the viscosity of the material in the mixing high-speed mixer increases and the temperature of the material rises, the mixing is stopped and the material is discharged for standby use;

[0028] (3) The mixed material is poured into a material barrel, and the internal mixer is started to set the heating temperature, and the material is poured in. After the material is evenly internally kneaded into a gel state, it is directly introduced into an extruder, and the four-stage mold temperature is set to a certain temperature, and the straw is extruded through a straw die head, and quickly cooled to room temperature with water. After the straw is shaped, it is air-dried with hot air, and finally cut into strips to obtain a biodegradable biomass-based straw, and then sterilized by UV ultraviolet rays and ozone, and then sealed and packaged.

[0029] Furthermore, in step (2), the material temperature is raised to 60-100° C. and mixing is stopped.

[0030] Furthermore, in step (3), the heating temperature of the internal mixer is set to 60-100°C, the four heating temperatures are 60-100°C, 80-125°C, 80-110°C and 80-120°C respectively, and the die temperature at the die outlet is 100-130°C.

[0031] The present invention has the following beneficial effects:

[0032] (1) The present invention uses waste biomass rice husks and shell powder as main raw materials, which are degradable materials, have low cost, save resources, are more environmentally friendly, and realize the recycling of biological waste;

[0033] (2) The biodegradable biomass-based straw provided by the present invention has good mechanical properties and hydrophobic properties, which can prolong the use time of the straw in water, effectively solving the problem that the straw becomes soft or even loose when it comes into contact with water during use, thus optimizing the use experience of the straw and having broad application prospects;

[0034] (3) The present invention can solve the problem of straws becoming moldy due to rapid growth of microorganisms caused by humid weather during transportation and storage; dopamine in the raw materials of the straws of the present invention has the effect of inhibiting bacterial growth, which can extend the storage time of the straws and improve safety;

[0035] (4) The present invention can solve the environmental pollution problem caused by non-degradable plastic straws and can completely replace most of the existing straws, thus having high social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings described herein are used to provide further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0037] in:

[0038] Figure 1 This is a picture of the finished product of the biomass-based straw of the present invention. DETAILED DESCRIPTION

[0039] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] Example 1

[0041] A process for preparing a degradable biomass-based straw comprises the following components in parts by weight:

[0042] 50 parts of rice husk powder with an average particle size of 100 mesh, 20 parts of shell powder with an average particle size of 200 mesh, 20 parts of polyhydroxyalkanoate (PHA), 10 parts of chitosan, 5 parts of tannic acid, 5 parts of hexadecyltrimethoxysilane (HDTMS) and 2 parts of dopamine. The preparation process of chitosan is as follows: add the washed chitosan (1g) to a 1mol / L hydrochloric acid solution and stir vigorously at 60 degrees for 3 hours. Then treat with 2mol / L sodium hydroxide to remove strongly bound proteins. Finally, centrifuge and wash, and dialyze the suspension until the pH is neutral. Finally, freeze-dry the suspension in a vacuum freeze dryer at minus 50°C for 12 hours to obtain chitosan.

[0043] A production process of biodegradable biomass-based straws, comprising the following steps:

[0044] (1) Weighing each raw material component by weight and adding them into a high-speed mixer for mixing;

[0045] (2) When the viscosity of the material in the mixing high-speed mixer increases and the material temperature rises to 60 degrees, the mixing is stopped and the material is discharged for standby use;

[0046] (3) Pour the mixed material into a material barrel, start an internal mixer and set the heating temperature to 60° C., pour the material obtained in step (2), and directly introduce the material into an extruder after uniform internal mixing into a gel state, set the four-stage mold temperature to 60° C., 80° C., 80° C. and 80° C. respectively, extrude the drawn strips through a straw die head, and set the die temperature of the die head outlet to 100° C. After rapid water cooling and shaping, air-dry it with hot air, and finally cut it into strips to obtain straws, and then sterilize it with UV ultraviolet rays and ozone, and then seal and package it.

[0047] Example 2

[0048] A process for preparing a degradable biomass-based straw comprises the following components in parts by weight:

[0049] 100 parts of rice husk powder with an average particle size of 200 mesh, 40 parts of shell powder with an average particle size of 400 mesh, 40 parts of polyhydroxyalkanoate (PHA), 20 parts of chitosan, 10 parts of tannic acid, 10 parts of hexadecyltrimethoxysilane (HDTMS) and 4 parts of dopamine. The preparation process of chitosan is as follows: add the washed chitosan (10g) to a 2mol / L hydrochloric acid solution and stir vigorously at 60 degrees for 4 hours. Then treat with 4mol / L sodium hydroxide to remove strongly bound proteins. Finally, centrifuge and wash, and dialyze the suspension until the pH is neutral. Finally, freeze-dry the suspension in a vacuum freeze dryer at minus 60°C for 16 hours to obtain chitosan.

[0050] A production process of biodegradable biomass-based straws, comprising the following steps:

[0051] (1) Weighing each raw material component by weight and adding them into a high-speed mixer for mixing;

[0052] (2) When the viscosity of the material in the mixing high-speed mixer increases and the material temperature rises to 80 degrees, the mixing is stopped and the material is discharged for standby use;

[0053] (3) Pour the mixed material into a material barrel, start the internal mixer and set the heating temperature to 60° C., pour the material obtained in step (2), and directly introduce the material into an extruder after uniform internal mixing into a gel state, set the four-stage mold temperature to 80° C., 100° C., 100° C. and 100° C. respectively, extrude the drawn strips through the straw die head, and the die temperature at the die outlet is 100° C. After rapid water cooling and shaping, dry it with hot air, and finally cut it into strips to obtain straws, and then sterilize it with UV ultraviolet rays and ozone, and then seal and package it.

[0054] Example 3

[0055] A process for preparing a degradable biomass-based straw comprises the following components in parts by weight:

[0056] 100 parts of rice husk powder with an average particle size of 100 mesh, 60 parts of shell powder with an average particle size of 200 mesh, 30 parts of polyhydroxyalkanoate (PHA), 10 parts of chitosan, 15 parts of tannic acid, 10 parts of hexadecyltrimethoxysilane (HDTMS) and 4 parts of dopamine. The preparation process of chitosan is as follows: add the washed shell (5g) to a 3mol / L hydrochloric acid solution and stir vigorously at 60 degrees for 4 hours. Then treat with 5mol / L sodium hydroxide to remove strongly bound proteins. Finally, centrifuge and wash, and dialyze the suspension until the pH is neutral. Finally, freeze-dry the suspension in a vacuum freeze dryer at minus 50°C for 16 hours to obtain chitosan.

[0057] A production process of biodegradable biomass-based straws, comprising the following steps:

[0058] (1) Weighing each raw material component by weight and adding them into a high-speed mixer for mixing;

[0059] (2) When the viscosity of the material in the mixing high-speed mixer increases and the material temperature rises to 80 degrees, the mixing is stopped and the material is discharged for standby use;

[0060] (3) Pour the mixed material into a material barrel, start the internal mixer and set the heating temperature to 80° C., pour the material obtained in step (2), and directly introduce the material into an extruder after uniform internal mixing into a gel state, set the four-stage mold temperature to 100° C., 80° C., 100° C. and 120° C. respectively, extrude the drawn strips through the straw die head, and the die temperature of the die head outlet is 110° C. After rapid water cooling and shaping, it is air-dried with hot air, and finally cut into strips to obtain straws, and then sterilized by UV ultraviolet rays and ozone, and then sealed and packaged.

[0061] Example 4

[0062] A process for preparing a degradable biomass-based straw comprises the following components in parts by weight:

[0063] 100 parts of rice husk powder with an average particle size of 500 mesh, 70 parts of shell powder with an average particle size of 2000 mesh, 20 parts of polyhydroxyalkanoate (PHA), 10 parts of chitosan, 25 parts of tannic acid, 10 parts of hexadecyltrimethoxysilane (HDTMS) and 2 parts of dopamine. The preparation process of chitosan is as follows: add the washed chitosan (10g) to a 4mol / L hydrochloric acid solution and stir vigorously at 60 degrees for 3 hours. Then treat with 8mol / L sodium hydroxide to remove strongly bound proteins. Finally, centrifuge and wash, and dialyze the suspension until the pH is neutral. Finally, freeze-dry the suspension in a vacuum freeze dryer at minus 70°C for 12 hours to obtain chitosan.

[0064] A production process of biodegradable biomass-based straws, comprising the following steps:

[0065] (1) Weighing each raw material component by weight and adding them into a high-speed mixer for mixing;

[0066] (2) When the viscosity of the material in the mixing high-speed mixer increases and the material temperature rises to 100 degrees, the mixing is stopped and the material is discharged for standby use;

[0067] (3) Pour the mixed material into a material barrel, start the internal mixer and set the heating temperature to 60° C., pour the material obtained in step (2), and directly introduce the material into an extruder after uniform internal mixing into a gel state, set the four-stage mold temperature to 60° C., 110° C., 110° C. and 110° C. respectively, extrude the drawn strips through the straw die head, and the die temperature at the die outlet is 120° C. After rapid water cooling and shaping, it is air-dried with hot air, and finally cut into strips to obtain straws, and then sterilized by UV ultraviolet rays and ozone, and then sealed and packaged.

[0068] Example 5

[0069] A process for preparing a degradable biomass-based straw comprises the following components in parts by weight:

[0070] 50 parts of rice husk powder with an average particle size of 800 mesh, 20 parts of shell powder with an average particle size of 1000 mesh, 20 parts of polyhydroxyalkanoate (PHA), 30 parts of chitosan, 20 parts of tannic acid, 10 parts of hexadecyltrimethoxysilane (HDTMS) and 2 parts of dopamine. The preparation process of chitosan is as follows: add the washed carapace (20g) to a 6mol / L hydrochloric acid solution and stir vigorously at 60 degrees for 3 hours. Then treat with 5mol / L sodium hydroxide to remove strongly bound proteins. Finally, centrifuge and wash, and dialyze the suspension until the pH is neutral. Finally, freeze-dry the suspension in a vacuum freeze dryer at minus 80°C for 12 hours to obtain chitosan.

[0071] A production process of biodegradable biomass-based straws, comprising the following steps:

[0072] (1) Weighing each raw material component by weight and adding them into a high-speed mixer for mixing;

[0073] (2) When the viscosity of the material in the mixing high-speed mixer increases and the material temperature rises to 100 degrees, the mixing is stopped and the material is discharged for standby use;

[0074] (3) Pour the mixed material into a material barrel, start an internal mixer and set the heating temperature to 100° C., pour the material obtained in step (2), and directly introduce the material into an extruder after uniform internal mixing into a gel state, set the four-stage mold temperature to 60° C., 125° C., 110° C. and 120° C. respectively, extrude the drawn strips through a straw die head, and set the die temperature at the die outlet to 130° C., quickly cool with water to shape, and then air-dry with hot air, finally cut into strips to obtain straws, and then sterilize them with UV ultraviolet rays and ozone, and then seal and package them.

[0075] Performance Testing

[0076] The properties of the biodegradable straws prepared in Examples 1-5 were measured, and the results are shown in Table 1.

[0077]

[0078] Table 1

[0079] The biodegradable straw obtained in Example 1 was subjected to degradation test, and the results are shown in Table 2:

[0080] Among them, test method: see IS014855-1:2012 / ASTM D5338-15(2021)

[0081] Reference material: Microcrystalline cellulose

[0082] Test container: The container used for biodegradation test is a high pressure conical flask, volume: 3000 ml

[0083]

[0084] Table 2

[0085] The biodegradable straw obtained in Example 1 was subjected to an antibacterial test, and the results are shown in Table 3:

[0086]

[0087] Note: Test method: Appendix C of GB / T21510-2008.

[0088] Table 3

[0089] It can be seen from Tables 1-3 above that the straws prepared by the process of the present invention have good physical properties and good degradation and antibacterial effects.

[0090] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A biodegradable biomass-based straw material, characterized in that: The materials of the degradable biomass-based straw include the following components by weight: 50-100 parts of rice husk powder; 20-70 parts of shell powder; 20-60 parts of polyhydroxyalkanoates; Chitosan 10-30 parts; Tannic acid 5-30 parts; 5-20 parts of hexadecyltrimethoxysilane; Dopamine 2-10 parts.

2. The biodegradable biomass-based straw material according to claim 1, characterized in that: The preparation process of the chitosan is as follows: (1) Add the cleaned carapace into a hydrochloric acid solution and stir vigorously at a certain temperature for 3-8 hours; (2) then treated with sodium hydroxide to remove strongly bound proteins; (3) centrifugation, washing, and dialyzing the suspension until the pH is neutral; (4) Freeze-drying the suspension in a vacuum freeze dryer to obtain chitosan.

3. The biodegradable biomass-based straw material according to claim 2, characterized in that: The carapace is the carapace of marine arthropods or insects, and the mass of the carapace is 1-20 g and the temperature is 60-120 degrees.

4. The biodegradable biomass-based straw material according to claim 2, characterized in that: The concentrations of the hydrochloric acid and the sodium hydroxide are 1-10 mol / L and 2-8 mol / L respectively; the temperature of the vacuum freeze dryer is minus 50-80° C., and the freezing time is 12-24 hours.

5. The biodegradable biomass-based straw material according to claim 1, characterized in that: The rice husk powder is agricultural waste generated in the rice production process, and its average particle size is 100-2000 meshes.

6. The biodegradable biomass-based straw material according to claim 1, characterized in that: The average particle size of the shell powder is 200 to 5000 meshes.

7. A process for preparing a degradable biomass-based straw, characterized in that: The steps include: (1) weighing rice husk powder, shell powder, chitosan, tannic acid, hexadecyltrimethoxysilane and dopamine in proportion, adding them into a high-speed mixer, mixing and stirring, then adding a certain amount of polyhydroxyalkanoate, and continuing to stir; (2) When the viscosity of the material in the mixing high-speed mixer increases and the temperature of the material rises, the mixing is stopped and the material is discharged for standby use; (3) The mixed material is poured into a material barrel, the internal mixer is started and set to a heating temperature, and the material is poured in. After the material is evenly internally kneaded into a gel state, it is directly introduced into an extruder, and the four-stage mold temperature is set to a certain temperature, and the straw is extruded through a straw die head, and quickly cooled to room temperature with water. After the straw is shaped, it is air-dried with hot air, and finally cut into strips to obtain a biodegradable biomass-based straw.

8. The process for preparing a degradable biomass-based straw material according to claim 7, characterized in that: In step (2), the material temperature is raised to 60-100° C. and mixing is stopped.

9. The process for preparing a degradable biomass-based straw material according to claim 7, characterized in that: In step (3), the heating temperature of the internal mixer is set to 60-100°C, the four heating temperatures are 60°C-100°C, 80°C-125°C, 80°C-110°C and 80°C-120°C respectively, the die temperature of the die discharge port is 100°C-130°C, and the obtained straws are sterilized by UV ultraviolet rays and ozone and then sealed and packaged.