Preparation method of biodegradable green printing ink

By using plasma to treat modified polylactic acid microspheres in the ink, the harm of non-degradable resin materials to the environment and high production costs of existing inks was solved, and a high adhesion fastness, good initial dryness and degradation rate were prepared. High biodegradable green printing ink achieves the goal of excellent performance and environmental protection.

CN119081472AActive Publication Date: 2024-12-06ZHEJIANG PUJIANG YONGTAI INK CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411366999.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

In the existing ink preparation technology, the non-degradable resin materials used are harmful to the environment and food, and have high production costs, which are neither economical nor environmentally friendly.

Method used

Polylactic acid microspheres are used as the main material, and limonene and biphenyl groups are introduced through plasma treatment. The modified microspheres are enhanced in interaction with the ink components, which improve the adhesion and dispersion of the ink, and mix and stir through a high-speed disperser. Uniformly prepare biodegradable green printing inks.

Benefits of technology

It significantly improves the adhesion, dispersion and wetting properties of the ink and enhances compatibility. The ink is almost completely degraded after 100 days, has excellent performance and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of biodegradable green printing ink, and belongs to the technical field of ink preparation. The preparation method comprises the following steps: uniformly mixing and stirring polylactic acid microspheres, isopropanol, a pigment, a defoaming agent, a flatting agent, a surfactant, ammonia water and deionized water in a high-speed dispersion machine to obtain the biodegradable green printing ink. The preparation method comprises the following steps: performing dehydration condensation on a lactic acid aqueous solution to obtain polylactic acid seed microspheres; stirring and mixing the polylactic acid seed microspheres, gamma-aminopropyltriethoxysilane, benzoyl peroxide and triethanolamine monooleate, adding di-tert-butyl methylphenol, and carrying out a swelling reaction to obtain polylactic acid microspheres; and taking the polylactic acid microspheres, placing the polylactic acid microspheres in low-temperature plasma treatment equipment, and carrying out plasma treatment on the polylactic acid microspheres, thereby obtaining the polylactic acid microspheres. The biodegradable green printing ink prepared by the invention is high in degradation rate, and is almost completely degraded after 100 days; the printing ink disclosed by the invention is high in adhesion fastness, good in initial dryness and excellent in comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ink preparation, in particular to a method for preparing biodegradable green printing ink. Background Art

[0002] At present, China has become the world's second largest ink producer, with hundreds of small and medium-sized manufacturing companies distributed across the country. At the same time, there are more than 200 water-based ink manufacturers, and only a handful of water-based ink manufacturers have an annual output of more than 1,000 tons. The domestic market demand for special printing inks such as lithographic offset inks, screen printing inks, and flexographic inks is on the rise, and as people's concept of sustainable development strengthens, the demand for more advanced environmentally friendly inks such as alcohol-soluble and water-based inks is also expected to grow rapidly.

[0003] Chinese patent CN115838547A: discloses a method for preparing water-based ink for PVC decorative film, which comprises, by weight: 2-6 parts of polyvinyl alcohol grinding resin, 10-18 parts of pigment, 1-3 parts of dispersant, 0.1-0.5 parts of defoamer, 20-35 parts of water-based epoxy resin, 0.5-1.5 parts of wetting agent, 1-2 parts of cosolvent, 13-40 parts of purified water, 1-1.5 parts of surfactant, 20-40 parts of water-based PVC glue, 1-3 parts of nano titanium dioxide dispersion, 0.5-1 parts of polyethylene wax powder, and 20-35 parts of ethyl acetate.

[0004] Chinese patent CN115449260A: relates to the field of ink processing, specifically discloses a water-based ink and its preparation method. A water-based ink includes a composite binder, the composite binder includes a modified epoxy resin, an acrylic resin and a silicone resin, and the mass ratio of the modified epoxy resin, acrylic resin and silicone resin is (1.2-2.0): (2.3-3.1): (0.8-1.9); its preparation method is: S1: prepare the composite binder; S2: add pigment, deionized water and surfactant to the mixed composite binder, stir well to obtain a matrix mixture; S3: add ammonia water, thickener, polyether modified polysiloxane defoamer, ink diluent, slow drying agent and candle agent to the matrix mixture in sequence, stir and mix, and finally obtain the water-based ink.

[0005] Chinese patent CN110669376A: discloses a general high-end water-based UV ink preparation method, which relates to the technical field of water-based ink preparation. It includes adding 40-55 parts of silicone-modified water-based polyurethane acrylate prepolymer and 20-30 parts of acrylate monomer into a stirring barrel, stirring at a stirring speed of 700-1000rpm for 10-20 minutes; transferring the pre-dispersed liquid to a grinder and grinding 1-3 times; transferring the ground liquid to a stirring barrel, adding 1-10 parts of photoinitiator, 5-10 parts of pigment, 5-15 parts of solvent and 1-5 parts of auxiliary agent into the stirring barrel, stirring at a stirring speed of 700-1000rpm for 20-30 minutes to mix the mixed liquid evenly, and obtaining a water-based UV ink.

[0006] The inks prepared by the above patents and prior art use non-degradable resin materials as binders, which are harmful to the environment, food, etc., and generally have high production costs, which are neither economical nor environmentally friendly. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a method for preparing a biodegradable green printing ink, and the operating steps are as follows:

[0008] 30-40 parts of polylactic acid microspheres, 10-15 parts of isopropyl alcohol, 10-15 parts of pigments, 1-3 parts of defoamers, 1-3 parts of leveling agents, 1-3 parts of surfactants, 1-5 parts of ammonia water and 15-25 parts of deionized water are mixed and stirred uniformly in a high-speed disperser to obtain biodegradable green printing ink.

[0009] As a preferred embodiment, the pigment is one of methyl orange, methyl blue, crystal violet, carbon black, titanium dioxide, magenta 6B, and benzidine yellow.

[0010] As a preferred embodiment, the defoaming agent is one of dimethyl polysiloxane, trimethyl silicone oil, mineral oil, emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether, and polydimethylsiloxane.

[0011] As a preferred embodiment, the leveling agent is one of BYK-378 leveling agent, hydroxymethyl cellulose, silicone oil, polydimethylsiloxane, polymethyl alkylsiloxane, polyether polyester modified organic siloxane, alkyl modified organic siloxane, and polyether modified dimethyl polysiloxane.

[0012] As a preferred embodiment, the surfactant is one of sodium dodecylbenzene sulfonate, sulfated castor oil, sodium dioctyl succinate sulfonate, sodium glycocholate, sodium oleate, and sodium lignin sulfonate.

[0013] As a preferred embodiment, the preparation method of the polylactic acid microspheres is:

[0014] A1: Dehydration condensation of lactic acid aqueous solution at 170-180°C to obtain polylactic acid seed microspheres;

[0015] A2: 60-90 parts of polylactic acid seed microspheres, 1-5 parts of γ-aminopropyl triethoxysilane, 1-3 parts of benzoyl peroxide, and 1-3 parts of triethanolamine monooleate are stirred and mixed, and then 1-3 parts of di-tert-butyl methylphenol are added to cause swelling reaction to obtain polylactic acid microspheres;

[0016] A3: Take 40-100 portions of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as a carrier gas, control the gas flow rate to 10-20 ml / min, and adjust the power to 100-200 watts, and perform plasma treatment on the polylactic acid microspheres for 30-60 minutes to obtain modified polylactic acid microspheres;

[0017] As a preferred solution, the mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide, and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.2-0.5:0.002-0.03.

[0018] Reaction mechanism

[0019] 1. Plasma modification to introduce amine groups

[0020] The polylactic acid microspheres are first treated with plasma to activate their surface to form free radicals or ions, which then react with amine-containing compounds (such as aminosilane coupling agents) to successfully introduce amine groups onto the surface of the microspheres; this process provides the necessary functional groups for subsequent chemical reactions.

[0021] 2. Ring-opening addition reaction of amine group and epoxy group

[0022] The amine groups introduced into the surface of the polylactic acid microspheres undergo a ring-opening addition reaction with the epoxy groups in (+)-limonene 1,2-epoxide; the amine groups act as nucleophiles to attack the carbon atoms on the epoxy ring, resulting in the opening of the ring and the formation of a new hydroxyl and secondary amine group, which means that the limonene group is covalently bonded to the surface of the microspheres.

[0023] 3. Mercapto-epoxy ring-opening addition reaction

[0024] The hydroxyl group formed in the second step can continue to undergo a ring-opening addition reaction with the thiol group in biphenyl-4,4'-dithiol; similarly, the thiol group acts as a nucleophile to attack the carbon atom next to the hydroxyl group, causing a ring opening and forming a new thioether bond to connect the biphenyl group, thus completing the surface functionalization of the polylactic acid microspheres.

[0025] Technical Effects

[0026] The present invention provides a method for preparing a biodegradable green printing ink. Compared with the prior art, the present invention has the following significant effects:

[0027] 1. Improve surface roughness and chemical diversity

[0028] By grafting limonene and biphenyl groups, the surface of the polylactic acid microspheres becomes rough and the chemical properties are more diverse; this physical and chemical change is conducive to enhancing the interaction with other components in the ink, including providing more possible hydrogen bonds and electrostatic attraction, thereby significantly improving the adhesion of the ink.

[0029] 2. Improve dispersibility and wettability

[0030] The increased surface polarity of the modified microspheres helps to improve their dispersibility and wettability in the ink; this is not only beneficial to the uniform distribution of the ink, but also helps to make the film layer uniform after drying, further promoting the improvement of ink adhesion.

[0031] 3. Enhanced compatibility

[0032] The introduced limonene and biphenyl groups increase the compatibility of polylactic acid microspheres with other organic components in the ink, reducing the possibility of phase separation; this increased compatibility is conducive to forming a uniform and stable ink system, thereby maintaining good adhesion during and after printing. DETAILED DESCRIPTION

[0033] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description in combination with embodiments and comparative examples:

[0034] 1. Adhesion fastness and initial drying test: refer to QB / T1046-2012 for testing;

[0035] 2. Degradation rate: The degradation rate of ink after 100 days of burial.

[0036] Example 1

[0037] A method for preparing a biodegradable green printing ink, the operating steps of which are:

[0038] 30 g of polylactic acid microspheres, 10 g of isopropyl alcohol, 10 g of pigment, 1 g of defoamer, 1 g of leveling agent, 1 g of surfactant, 1 g of ammonia water, and 15 g of deionized water were mixed and stirred uniformly in a high-speed disperser to obtain a biodegradable green printing ink.

[0039] The pigment is methyl orange.

[0040] The defoaming agent is dimethyl polysiloxane.

[0041] The leveling agent is BYK-378 leveling agent.

[0042] The surfactant is sodium dodecylbenzene sulfonate.

[0043] The preparation method of the polylactic acid microspheres is:

[0044] A1: Dehydration condensation of L-lactic acid (L-LA) aqueous solution at 170°C to obtain polylactic acid seed microspheres;

[0045] A2: 60 g of polylactic acid seed microspheres, 1 g of γ-aminopropyl triethoxysilane, 1 g of benzoyl peroxide, and 1 g of triethanolamine monooleate were stirred and mixed, and then 1 g of di-tert-butyl methylphenol was added to cause swelling reaction to obtain polylactic acid microspheres;

[0046] A3: Take 40g of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as the carrier gas, control the gas flow rate at 10 ml / min, and adjust the power to 100 watts, and perform plasma treatment on the polylactic acid microspheres for 30 minutes to obtain modified polylactic acid microspheres.

[0047] The mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.2:0.002.

[0048] Example 2

[0049] A method for preparing a biodegradable green printing ink, the operating steps of which are:

[0050] 33 g of polylactic acid microspheres, 12 g of isopropyl alcohol, 12 g of pigment, 2 g of defoamer, 2 g of leveling agent, 2 g of surfactant, 2 g of ammonia water, and 18 g of deionized water were mixed and stirred uniformly in a high-speed disperser to obtain a biodegradable green printing ink.

[0051] The pigment is methyl blue.

[0052] The defoaming agent is trimethyl silicone oil.

[0053] The leveling agent is hydroxymethyl cellulose.

[0054] The surfactant is sulfated castor oil.

[0055] The preparation method of the polylactic acid microspheres is:

[0056] A1: Dextrorotatory lactic acid (D-LA) aqueous solution was dehydrated and condensed at 175°C to obtain polylactic acid seed microspheres;

[0057] A2: 70 g of polylactic acid seed microspheres, 2 g of γ-aminopropyl triethoxysilane, 2 g of benzoyl peroxide, and 2 g of triethanolamine monooleate were stirred and mixed, and then 2 g of di-tert-butyl methylphenol was added to cause swelling reaction to obtain polylactic acid microspheres;

[0058] A3: Take 60g of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as the carrier gas, control the gas flow rate at 15 ml / min, and adjust the power to 140 watts, and perform plasma treatment on the polylactic acid microspheres for 40 minutes to obtain modified polylactic acid microspheres.

[0059] The mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide, and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.3:0.01.

[0060] Example 3

[0061] A method for preparing a biodegradable green printing ink, the operating steps of which are:

[0062] 38 g of polylactic acid microspheres, 14 g of isopropyl alcohol, 14 g of pigment, 2 g of defoamer, 2 g of leveling agent, 2 g of surfactant, 4 g of ammonia water, and 23 g of deionized water were mixed and stirred uniformly in a high-speed disperser to obtain a biodegradable green printing ink.

[0063] The pigment is crystal violet.

[0064] The defoaming agent is mineral oil.

[0065] The leveling agent is silicone oil.

[0066] The surfactant is dioctyl sodium sulfosuccinate.

[0067] The preparation method of the polylactic acid microspheres is:

[0068] A1: dehydration condensation of racemic lactic acid (DL-LA) aqueous solution at 175°C to obtain polylactic acid seed microspheres;

[0069] A2: 80 g of polylactic acid seed microspheres, 4 g of γ-aminopropyl triethoxysilane, 2 g of benzoyl peroxide, and 2 g of triethanolamine monooleate were stirred and mixed, and then 2 g of di-tert-butyl methylphenol was added to cause swelling reaction to obtain polylactic acid microspheres;

[0070] A3: Take 80g of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as the carrier gas, control the gas flow rate at 15 ml / min, and adjust the power to 180 watts, and perform plasma treatment on the polylactic acid microspheres for 50 minutes to obtain modified polylactic acid microspheres.

[0071] The mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.4:0.02.

[0072] Example 4

[0073] A method for preparing a biodegradable green printing ink, the operating steps of which are:

[0074] 40 g of polylactic acid microspheres, 15 g of isopropyl alcohol, 15 g of pigment, 3 g of defoamer, 3 g of leveling agent, 3 g of surfactant, 5 g of ammonia water, and 25 g of deionized water were mixed and stirred uniformly in a high-speed disperser to obtain a biodegradable green printing ink.

[0075] The pigment is carbon black.

[0076] The defoaming agent is polydimethylsiloxane.

[0077] The leveling agent is polyether modified dimethyl polysiloxane.

[0078] The surfactant is sodium lignin sulfonate.

[0079] The preparation method of the polylactic acid microspheres is:

[0080] A1: dehydration condensation of racemic lactic acid (DL-LA) aqueous solution at 180°C to obtain polylactic acid seed microspheres;

[0081] A2: 90 g of polylactic acid seed microspheres, 5 g of γ-aminopropyl triethoxysilane, 3 g of benzoyl peroxide, and 3 g of triethanolamine monooleate were stirred and mixed, and then 3 g of di-tert-butyl methylphenol was added to cause swelling reaction to obtain polylactic acid microspheres;

[0082] A3: Take 100g of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as the carrier gas, control the gas flow rate at 20 ml / min, and adjust the power to 200 watts, and perform plasma treatment on the polylactic acid microspheres for 60 minutes to obtain modified polylactic acid microspheres.

[0083] The mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide, and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.5:0.03.

[0084] Comparative Example 1

[0085] The polylactic acid microspheres were not modified, and the other steps were the same as in Example 1.

[0086] Comparative Example 2

[0087] The other steps were the same as in Example 1 except that (+)-limonene 1,2-epoxide was not added.

[0088] Comparative Example 3

[0089] The other steps were the same as in Example 1 except that biphenyl-4,4'-dithiol was not added.

[0090] Adhesion fastness / % Initial drying / mm / 30s Degradation rate / % Example 1 91 39 93 Example 2 94 37 95 Example 3 96 35 98 Example 4 97 34 100 Comparative Example 1 68 66 69 Comparative Example 2 82 49 85 Comparative Example 3 85 46 88

[0091] Through the data analysis of the above embodiments and comparative examples, the ink prepared by the present invention has a high degradation rate and is almost completely degraded after 100 days. It is an ink material with excellent performance and environmental friendliness; the biodegradable green printing ink prepared by the present invention has high adhesion fastness, good initial drying property, and excellent comprehensive performance of the ink.

[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a biodegradable green printing ink, the operating steps of which are: 30-40 parts of polylactic acid microspheres, 10-15 parts of isopropyl alcohol, 10-15 parts of pigments, 1-3 parts of defoamers, 1-3 parts of leveling agents, 1-3 parts of surfactants, 1-5 parts of ammonia water and 15-25 parts of deionized water are mixed and stirred uniformly in a high-speed disperser to obtain biodegradable green printing ink.

2. The method for preparing a biodegradable green printing ink according to claim 1, characterized in that: The pigment is one of methyl orange, methyl blue, crystal violet, carbon black, titanium dioxide, magenta 6B and benzidine yellow.

3. The method for preparing a biodegradable green printing ink according to claim 1, characterized in that: The defoaming agent is one of dimethyl polysiloxane, trimethyl silicone oil, mineral oil, emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropanolamine ether, polyoxypropylene glycerol ether, polyoxypropylene polyoxyethylene glycerol ether, and polydimethylsiloxane.

4. The method for preparing a biodegradable green printing ink according to claim 1, characterized in that: The leveling agent is one of BYK-378 leveling agent, hydroxymethyl cellulose, silicone oil, polydimethylsiloxane, polymethyl alkylsiloxane, polyether polyester modified organic siloxane, alkyl modified organic siloxane and polyether modified dimethyl polysiloxane.

5. The method for preparing a biodegradable green printing ink according to claim 1, characterized in that: The surfactant is one of sodium dodecylbenzene sulfonate, sulfated castor oil, dioctyl sodium succinate sulfonate, sodium glycocholate, sodium oleate and sodium lignin sulfonate.

6. The method for preparing a biodegradable green printing ink according to claim 1, characterized in that: The preparation method of the polylactic acid microspheres is: A1: Dehydration condensation of lactic acid aqueous solution at 170-180°C to obtain polylactic acid seed microspheres; A2: 60-90 parts of polylactic acid seed microspheres, 1-5 parts of γ-aminopropyl triethoxysilane, 1-3 parts of benzoyl peroxide, and 1-3 parts of triethanolamine monooleate are stirred and mixed, and then 1-3 parts of di-tert-butyl methylphenol are added to cause swelling reaction to obtain polylactic acid microspheres; A3: Take 40-100 portions of polylactic acid microspheres and place them in a low-temperature plasma treatment device; select mixed steam as the carrier gas, control the gas flow rate at 10-20 ml / min, and adjust the power to 100-200 watts, and perform plasma treatment on the polylactic acid microspheres for 30-60 minutes to obtain modified polylactic acid microspheres.

7. The method for preparing a biodegradable green printing ink according to claim 6, characterized in that: The mixed steam is a mixed steam of ammonia, (+)-limonene 1,2-epoxide and biphenyl-4,4'-dithiol CAS No. 6954-27-4, with a volume ratio of 1:0.2-0.5:0.002-0.03.

Citation Information

Patent Citations

  • Method for hydrophilization modification of polylactic acid fibres

    CN103015174A

  • Polylactic acid photo / hydrolytic-double-degradable polymer and preparation method thereof

    CN104910361A

  • Full-degradable polymer stent with surface adhered with drug coating layer and preparation method of full-degradable polymer stent

    CN107137790A

  • High molecular material surface modification method and its product and application

    CN107189096A

  • Biodegradable green printing ink binder and ink

    CN110128642A