Single-component water-based multifunctional transparent matte finish paint and preparation method thereof

By using combination components such as self-crosslinking emulsions and cage-type polysilsesquioxane-modified vapor phase silica in water-based wood paint, the wear resistance and scratch resistance caused by the floating of matting powder in existing water-based wood paints is solved. The stability and uniformity of the topcoat are achieved, and the wear resistance and scratch resistance of the coating are improved.

CN119081491APending Publication Date: 2024-12-06KUNSHAN AICA KOGYO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410975378.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When the existing water-based wood paint improves the matteness of the topcoat, the floating of the matting powder leads to poor wear resistance and scratch resistance, and is difficult to control the viscosity, which easily leads to problems of fog and uneven gloss, affecting the stability and good products of the product. Rate.

Method used

Use a single-component water-based multifunctional transparent matte topcoat, through self-crosslinking lotion, deionized water, matte lotion, fungicide, wetting agent, dispersing agent, defoaming agent, antifreeze agent, film forming additive, The combination of solvent, anti-deposition agent, anti-scratch agent and light stabilizer controls the viscosity and surface tension of the topcoat to form a thickening and anti-deposition structure, reduces the amount of matte emulsion, and improves the wear resistance and durability of the coating. The dispersion and shrinkage of the topcoat are adjusted by cage polysilsesquioxane modification of the vapor phase silica.

Benefits of technology

The stability and uniformity of the topcoat are achieved, the wear resistance and scratch resistance of the coating are improved, the fog and uneven gloss are avoided, and the product is guaranteed to be stable and the product yield is obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954379250000091
    Figure BDA0004954379250000091
Patent Text Reader

Abstract

The invention relates to the field of water-based finish paint, and particularly discloses single-component water-based multifunctional transparent matte finish paint and a preparation method thereof. Comprising the following raw materials in parts by weight: 60 to 70 parts of a self-crosslinking emulsion, 10 to 20 parts of deionized water, 8 to 20 parts of a matte emulsion, 0.05 to 0.50 part of a bactericide, 0.1 to 0.5 part of a wetting agent, 0.4 to 0.8 part of a dispersant, 0.05 to 0.25 part of a defoaming agent, 0.5 to 1.0 part of an anti-freezing agent, 2 to 5 parts of a coalescing agent, 0.5 to 1 part of a solubilizer, 0.8 to 1.5 parts of an anti-settling agent, 0.2 to 1.0 part of an anti-scratch agent, 0.2 to 2.0 parts of a light stabilizer and 0.2 to 2.0 parts of a thickening agent. The anti-scratch agent comprises one or two of a flatting agent and a slipping agent. The water-based finish paint prepared by the invention has a relatively good scratch-resistant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of water-based topcoats, and more specifically, to a one-component water-based multifunctional transparent matte topcoat and a construction process thereof. Background Art

[0002] As people pay more and more attention to environmental protection and health, the market for water-based paint for wood is growing. At present, water-based wood paint with acrylic acid as the main component mainly improves the matte property of the topcoat by adding matting powder. However, after the matting powder floats, the wear resistance and scratch resistance of the topcoat are poor. The friction and collision of the product easily lead to surface glossiness. In addition, there are problems such as difficulty in dispersing wax emulsion and easy agglomeration. The viscosity of the overall varnish is required to be high. If the viscosity is not well controlled, it is easy to cause stratification and poor processability. The obtained product will have fog or uneven gloss, resulting in a decrease in the yield of the product. If the amount of matting powder is reduced, the matting effect will be affected. How to provide a water-based topcoat with stable components that are not easy to migrate and has good wear resistance and durability is a problem to be solved. Summary of the invention

[0003] In order to solve the problem of wear resistance and durability of water-based topcoats, the present application provides a one-component water-based multifunctional transparent matte topcoat.

[0004] In the first aspect, the present application provides a one-component water-based multifunctional transparent matte topcoat, which adopts the following technical scheme: a one-component water-based multifunctional transparent matte topcoat, comprising the following raw materials in parts by weight: 60-70 parts of self-cross-linking emulsion, 10-25 parts of deionized water, 8-20 parts of matte emulsion, 0.05-0.50 parts of bactericide, 0.1-0.5 parts of wetting agent, 0.4-0.8 parts of dispersant, 0.05-0.25 parts of defoaming agent, 0.5-1.0 parts of antifreeze agent, 2-5 parts of film-forming aid, 0.5-1 parts of solubilizer, 0.8-1.5 parts of anti-scratch agent, 0.2-1.0 parts of anti-scratch agent, 0.2-2.0 parts of light stabilizer, and 0.2-2.0 parts of thickener, wherein the anti-scratch agent includes one or both of a leveling agent and a lubricant.

[0005] By controlling the component selection and quality of the topcoat, the matte topcoat obtained has a thickening and anti-precipitation structure, suitable viscosity, good stability and uniformity of the product, and the matte emulsion is not easy to float. The topcoat product obtained has no fog and uniform gloss. The resin matting system of the topcoat can effectively improve the wear resistance and scratch resistance of the coating, improve the durability of the coating and make the gloss continue to be stable. Through thixotropy and leveling balance, when the topcoat of the present application is formed into a film, the system forms a microscopic concave and convex surface due to the change of surface tension, so that the coated substrate has a relatively dumb gloss, reducing the amount of matte emulsion, and further improving the wear resistance of the topcoat.

[0006] Water-based pure acrylic emulsion has wide applicability and good weather resistance. Silicone acrylic emulsion film is not easy to yellow, stable in water, film particle molecular tensile force is tight, strong flexibility, good wear resistance. Through the selection of self-crosslinking emulsion, the prepared topcoat has suitable viscosity, good weather resistance, relatively stable, components are not easy to phase separate, the formed topcoat surface tension is suitable, and it is more durable under the combination of the components of this application.

[0007] Preferably, the bactericide includes one or two of dibromocyanoacetamide and isothiazolinone solutions; Preferably, the wetting agent comprises an alkoxylated branched fatty alcohol having an HLB value of 12-14; Preferably, the dispersant includes one or both of a polycarboxylic acid ammonium salt dispersant and a polycarboxylic acid sodium salt dispersant; Preferably, the defoamer includes one or more of a mineral oil carrier polyether-modified fatty acid derivative defoamer or a polyether-modified silicone defoamer; Preferably, the antifreeze agent comprises propylene glycol; Preferably, the film-forming aid includes 2,2,4-trimethyl-1,3-pentanediol isobutyrate; Preferably, the solubilizer includes polyethylene glycol, PEG300-PEG500, to further improve the dispersibility and stability of the anti-settling agent; Preferably, the anti-scratch agent includes one or more of a methylsiloxane leveling agent or a methylsiloxane slip agent; Preferably, the light stabilizer includes one or both of bis-sebacate and 1-methyl-8-sebacate.

[0008] By adopting the above scheme, the prepared topcoat has good wetting and dispersibility, less foaming, no large foam, suitable viscosity of the system, and good processing effect.

[0009] In a specific embodiment, the self-crosslinking emulsion includes one or more of an aqueous pure acrylic or silicone acrylic emulsion.

[0010] The raw materials of water-based pure acrylic or silicone acrylic emulsion are easily available, relatively stable, and convenient to process, and are suitable for use in the matte topcoat prepared in this application.

[0011] In a specific embodiment, the self-crosslinking emulsion is an aqueous pure acrylic or silicone acrylic emulsion with a viscosity of 50-500 mPa×S.

[0012] By limiting the viscosity of pure acrylic emulsion or silicone acrylic emulsion, the components in the topcoat are evenly distributed, the amount of anti-settling agent and thickener is reduced, and the topcoat is relatively stable, not easy to stratify and produce fog, and the surface of the topcoat will not be rough due to excessive particle size. By limiting the viscosity of water-based pure acrylic emulsion / silicone acrylic emulsion, the matte emulsion in the topcoat is not easy to precipitate and float, and has good integration with the system, and the topcoat has better wear resistance and scratch resistance.

[0013] In a specific embodiment, the matte emulsion comprises an aqueous acrylic microsphere emulsion.

[0014] By adopting the above technical scheme, the water-based acrylic microsphere emulsion and the system emulsion form large and small particle size extinction, improve the matte property of the topcoat, the water-based acrylic microsphere emulsion has good compatibility with the water-based pure acrylic emulsion and the silicone acrylic emulsion, and is evenly dispersed. The prepared topcoat is more uniform and smooth, with stable gloss, and has low viscosity requirements for the overall topcoat, which is easy to apply. In the film-forming process, the acrylic emulsion microspheres will not spread and form a film along with the main film-forming material, and have good binding properties with the one-component acrylic system, avoiding abnormal wear resistance and scratch resistance of the product caused by floating.

[0015] In a specific embodiment, the anti-settling agent is hydrophilic nano-fumed silica, and the thickener is a non-ionic polyurethane thickener.

[0016] By adopting the above technical scheme, the fumed silica has a small particle size and a large specific surface area, and can interact with adjacent fumed silica particles to form hydrogen bonds, making the prepared topcoat more uniform and stable, preventing the floating of acrylic microspheres of the matting agent, and making the prepared topcoat more stable. The hydrophilic nano-fumed silica has good dispersibility with the system, effectively improving the wettability and interface bonding strength between the topcoat molecules, improving the comprehensive performance of the topcoat, and having a good anti-settling effect on the topcoat of this system. The prepared topcoat forms a microscopic concave and convex surface due to the change in surface tension when the single component forms a film through thixotropy and leveling balance, so that the product has a duller luster. The molecular hydrophobic end of the non-ionic polyurethane thickener associates with the hydrophobic structure in the topcoat, and the hydrophilic end thickens with water molecules through hydrogen bonds to form a three-dimensional network structure. The thickener and the anti-settling agent work together to make the prepared topcoat more uniform and stable, and the prepared topcoat has better wear resistance.

[0017] Preferably, the mass ratio of water-based nano-fumed silica to non-ionic polyurethane thickener is 1:1.2.

[0018] The applicant has found that by using hydrophilic nano-fumed silica and non-ionic polyurethane thickener in a certain mass ratio, the prepared topcoat is uniform and stable, has good thickening and anti-precipitation effects, is not too viscous to make construction difficult, and does not precipitate and stratify to affect the color and wear resistance of the topcoat. The prepared topcoat is smooth and uniform with good stability.

[0019] In a specific embodiment, the matte topcoat further comprises the following raw materials in parts by weight: 5-12 parts of cage-type polysilsesquioxane-modified fumed silica.

[0020] By adopting the above technical solution, cage-type polysilsesquioxane is a lightweight, high-performance material with a "cage-type" framework structure. By modifying fumed silica with cage-type polysilsesquioxane, the thickening effect of the topcoat is further adjusted. The fumed silica thickener has better dispersibility and compatibility in the coating, and may also play a similar "stirring" effect to make the prepared topcoat very uniform. The special structure of cage-type polysilsesquioxane also has good elasticity. When the topcoat is subjected to external force, the particles can terminate the development of microcrack tips, induce silver streaks and shear bands, and drive the rearrangement of fumed silica. The interpenetrating network between the fumed silica and the matrix formed by hydrogen bonding further disperses the stress, further improving the mechanical properties and dimensional stability of the topcoat, and it is not easy to be scratched when subjected to external friction. At the same time, the shrinkage of the topcoat was adjusted. The cage-type polysilsesquioxane-modified fumed silica has a large shrinkage rate, which further improves the matte effect of the topcoat after curing, further reduces the use of matting agents, and avoids the floating of matting agents that affects the wear resistance of the topcoat, thereby achieving a stable matte effect.

[0021] In a specific embodiment, the cage polysilsesquioxane is an amino cage polysilsesquioxane.

[0022] By adopting the above technical solution, the cage-type polysilsesquioxane is amino cage-type polysilsesquioxane, which is more evenly dispersed in the topcoat, and the compatibility of the system is better, and the improvement effect on the overall stability and wear resistance of the topcoat is more obvious.

[0023] In a specific embodiment, the mass ratio of the self-crosslinking latex to the cage-type polysilsesquioxane-modified fumed silica is 6:1.

[0024] At this mass ratio, the topcoat has a more obvious scratch resistance performance, which may be due to the better "interpenetrating network" structure formed in the topcoat system at this time.

[0025] In a second aspect, the present application provides a method for preparing a one-component water-based multifunctional transparent matte topcoat, characterized in that it comprises the following steps: S1. Mix deionized water and a dispersant, a wetting agent, a bactericide, a film-forming agent, and an antifreeze agent, and then add an anti-settling agent and stir and disperse at high speed for 25-35 minutes to form a mixed slurry; S2. Add the mixed slurry and matte emulsion to the self-crosslinking emulsion simultaneously, stir at medium speed for 8-12 minutes, and stir evenly to obtain the initial coating; S3. Add the remaining components, stir at a low speed for 3-8 minutes, then degas for 3-8 minutes, filter and fill to obtain a one-component water-based multifunctional transparent matte topcoat.

[0026] The topcoat prepared by the above steps can be mixed evenly in a shorter time, fewer bubbles are introduced into the topcoat, the components of the prepared topcoat are evenly distributed, not easy to precipitate, and the topcoat has good wear resistance and gloss performance.

[0027] In a specific embodiment, the high-speed stirring speed described in S1 is ≥1501 rpm; the medium-speed stirring speed described in S2 is 1001-1500 rpm; and the low-speed stirring speed described in S3 is ≤1000 rpm.

[0028] By adopting the above technical scheme, the preparation method is relatively simple, the requirements for the process are low, the prepared topcoat emulsion particles are relatively uniform, do not produce much foam, form a relatively stable structure, are not easy to produce precipitation, there is no haze after the topcoat is cured, and the wear resistance is good.

[0029] In summary, this application has the following beneficial effects: 1. Since the present application has a thickening and anti-precipitation structure, the product has good stability and uniformity. By designing the matting system of the topcoat, the wear resistance and scratch resistance of the coating are improved, and the gloss is sustained and stable. By forming large and small particle size matting for the system emulsion and acrylic microsphere emulsion, the abnormal wear resistance and scratch resistance of the product caused by the floating of the matting agent is solved. Through the combination of special thickeners and fumed silica, the system has a microscopic local network structure under low shear, which effectively solves the product haze and uneven gloss caused by the phase separation of wax emulsions or transparent pigments in the system. The product uses thixotropy and leveling balance, so that when a single component is formed into a film, the system forms a microscopic concave and convex surface due to changes in surface tension, which makes the product have a matte gloss.

[0030] 2. The present application adds cage-type polysilsesquioxane-modified fumed silica to the topcoat to improve the dispersibility of the topcoat, induce silver streaks and shear bands, and drive the fumed silica to rearrange to resist scratches. It also adjusts the shrinkage of the components to improve the matte effect and reduce the amount of matting agent. The resulting topcoat has good stability and scratch resistance. DETAILED DESCRIPTION

[0031] The self-crosslinking emulsion in Example 4 is pure acrylic emulsion from Shenhong Chemical Co., Ltd., and the other self-crosslinking emulsions are pure acrylic emulsion BLJ-960 from Baolijia; the matte emulsion in Example 9 is stearic acid emulsion WE-9410 from Shanghai Xinnuo Chemical, and the other matte emulsions are Dow's water-based acrylic microsphere emulsion OPTI-MATT TMAB-2; the amino cage polysilsesquioxane is aminoaminopropylheptyl POSS from Fossman Technology Co., Ltd.; the wetting agent is Dow CA-90; the bactericide is dibromocyanoacetamide purchased from Heze Runxin Biotechnology Co., Ltd.; the dispersant is Dongguan Leading Environmental Protection Material LX-5029 polycarboxylic acid amino salt type dispersant; the defoamer is the polyether modified silicone defoamer DU-1211 from Guozhong Research Institute; the antifreeze agent is propylene glycol; the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol isobutyrate; the solubilizer is PEG300; the anti-settling agent is hydrophilic nano-fumed silica; the anti-scratch agent is Digo 482; the light stabilizer is disebacate; the thickener is Qingtian New Material DH-7216S; the silane coupling agent is KH-550; and the antioxidant is antioxidant 1098.

[0032] The present application is further described in detail below in conjunction with the examples. Unless otherwise specified, the experimental reagents in the preparation examples and examples are all conventional commercial brands or obtained through conventional preparation processes.

[0033] Preparation Example Preparation Example 1: Amino cage polysilsesquioxane modified fumed silica 25 g of fumed silica and 20 g of amino cage polysilsesquioxane were added to 150 ml of 25% ethanol aqueous solution, stirred at 80° C. for 1 hour, repeatedly pumped and charged with nitrogen three times, ultrasonically treated for 80 minutes, reacted at 80° C. for 60 hours under stirring, and the excess cage polysilsesquioxane was removed by vacuum distillation, filtered, washed, and vacuum dried at 80° C. for 24 hours to obtain amino cage polysilsesquioxane-modified fumed silica.

[0034] Preparation Example 2: Aminosilane-modified fumed silica S1: Mix 3g of silane coupling agent, 200g of ethanol and 50g of pure water, stir evenly to obtain a mixed solution; S2: 120 g of fumed silica was added to the mixed solution obtained in S1, stirred at 80° C. for 1 hour, filtered, and dried to obtain aminosilane-modified fumed silica. Example

[0035] Example 1 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 60g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, and 23g of deionized water.

[0036] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0037] Example 2 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 65g of self-crosslinking emulsion, 15g of matte emulsion, 3g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.5g of thickener, and 23g of deionized water.

[0038] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0039] Example 3 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 70g of self-crosslinking emulsion, 20g of matte emulsion, 5g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.2g of thickener, and 23g of deionized water.

[0040] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0041] Example 4 The only difference between this embodiment and embodiment 1 is that the self-crosslinking emulsion is a pure acrylic emulsion produced by Shenhong Chemical Co., Ltd., and the viscosity is 1000-4000 mPa×S.

[0042] Example 5 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 60g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, 23g of deionized water, and 10g of amino cage-type polysilsesquioxane modified fumed silica obtained in Preparation Example 1.

[0043] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0044] Example 6 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 60g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, 23g of deionized water, and 10g of aminosilane-modified fumed silica obtained in Preparation Example 2.

[0045] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0046] Example 7 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 60g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, 23g of deionized water, 8g of amino cage polysilsesquioxane modified fumed silica prepared in Preparation Example 1, and 2g of aminosilane modified fumed silica prepared in Preparation Example 2.

[0047] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0048] Example 8 The difference between this embodiment and embodiment 1 is that the matte emulsion is Shanghai Xinnuo Chemical Stearic Acid Emulsion WE-9410.

[0049] Example 9 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 60g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, and 23g of deionized water.

[0050] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 1200 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0051] Comparative Example Comparative Example 1 The water-based multifunctional transparent matte topcoat of this embodiment is composed of the following raw materials in weight percentage: 50g of self-crosslinking emulsion, 8g of matte emulsion, 2g of film-forming aid, 1g of antifreeze agent, 0.5g of solubilizer, 1g of anti-settling agent, 0.5g of anti-scratch agent, 1g of light stabilizer, 0.5g of dispersant, 0.1g of wetting agent, 0.35g of bactericide, 0.2g of defoamer, 0.8g of thickener, and 23g of deionized water.

[0052] The preparation method is: S1. The deionized water and dispersant, wetting agent, fungicide, film-forming agent, antifreeze agent were mixed, an anti-settling agent was added, and the mixture was stirred and dispersed at 1600 rpm for 30 minutes to form a mixed slurry; S2. The mixed slurry and matte emulsion were added to the self-crosslinking emulsion three times simultaneously and stirred at 1200 rpm for 10 minutes to obtain an initial coating; S3. Add the remaining components to the initial coating, stir at 550 rpm for 5 minutes, degas for 5 minutes after stirring evenly, filter and fill to obtain a matte topcoat.

[0053] Performance test test 1: The wear resistance of each embodiment and comparative example was tested according to the method of standard GB / T1768-2006, with a load of 1000g and 500 revolutions. The test results are summarized in Table 1.

[0054] Test 2: The artificial aging resistance of each embodiment and comparative example was tested according to the method of standard GB / T14522-2008. The test results are summarized in Table 1.

[0055] Test 3: Reference standard GB / T 9279.1-2015 Determination of scratch resistance of paints and varnishes Part 1: Constant load method The artificial aging resistance of each embodiment and comparative example was tested. The test environment temperature was 25°C and the relative humidity was 50%; the test type was "pass / fail" and the test results were summarized in Table 1.

[0056] Table 1 It can be seen from Examples 1-4, Examples 8-9 and Comparative Example 1 and Table 1 that the matte topcoat prepared by the component ratio, viscosity and preparation steps of the present application has good scratch resistance and durability.

[0057] It can be seen from Example 1, Examples 5-7 and Table 1 that the matte topcoat prepared by adding a certain mass proportion of amino cage polysilsesquioxane modified fumed silica in the present application has good scratch resistance and durability.

[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A one-component water-based multifunctional transparent matte topcoat, characterized in that: The invention comprises the following raw materials in parts by weight: 60-70 parts of self-crosslinking emulsion, 10-25 parts of deionized water, 8-20 parts of matte emulsion, 0.05-0.50 parts of bactericide, 0.1-0.5 parts of wetting agent, 0.4-0.8 parts of dispersant, 0.05-0.25 parts of defoaming agent, 0.5-1.0 parts of antifreeze agent, 2-5 parts of film-forming aid, 0.5-1 parts of solubilizer, 0.8-1.5 parts of anti-scratch agent, 0.2-1.0 parts of anti-scratch agent, 0.2-2.0 parts of light stabilizer and 0.2-2.0 parts of thickener. The anti-scratch agent comprises one or both of leveling agent and lubricant.

2. The one-component water-based multifunctional transparent matte topcoat according to claim 1, characterized in that: The self-crosslinking emulsion includes one or more of water-based pure acrylic or silicone acrylic emulsions.

3. The one-component water-based multifunctional transparent matte topcoat according to claim 1, characterized in that: The self-crosslinking emulsion is a water-based pure acrylic or silicone acrylic emulsion with a viscosity of 50-500 mPa×S.

4. The one-component water-based multifunctional transparent matte topcoat according to claim 1, characterized in that: The matte emulsion includes water-based acrylic microsphere emulsion.

5. The one-component water-based multifunctional transparent matte topcoat according to claim 1, characterized in that: The anti-settling agent includes hydrophilic nano-gas phase silica, and the thickener includes a non-ionic polyurethane thickener.

6. The one-component water-based multifunctional transparent matte topcoat according to claim 1, characterized in that: The matte topcoat further comprises the following raw materials in parts by weight: 5-12 parts of cage-type polysilsesquioxane-modified fumed silica.

7. The one-component water-based multifunctional transparent matte topcoat according to claim 6, characterized in that: The cage-type polysilsesquioxane is an amino cage-type polysilsesquioxane.

8. The one-component water-based multifunctional transparent matte topcoat according to claim 6, characterized in that: The mass ratio of the self-crosslinking emulsion to the cage-type polysilsesquioxane-modified fumed silica is 6:

1.

9. A method for preparing the one-component water-based multifunctional transparent matte topcoat according to any one of claims 1 to 8, characterized in that: The steps include: S1. Mix deionized water and a dispersant, a wetting agent, a bactericide, a film-forming agent, and an antifreeze agent, and then add an anti-settling agent and stir and disperse at high speed for 25-35 minutes to form a mixed slurry; S2. Add the mixed slurry and matte emulsion to the self-crosslinking emulsion simultaneously, stir at medium speed for 8-12 minutes, and stir evenly to obtain the initial coating; S3. Add the remaining components, stir at a low speed for 3-8 minutes, then degas for 3-8 minutes, filter and fill to obtain a one-component water-based multifunctional transparent matte topcoat.

10. The method for preparing a one-component water-based multifunctional transparent matte topcoat according to claim 9, characterized in that: The high-speed stirring speed described in S1 is ≥1501 rpm; the medium-speed stirring speed described in S2 is 1001-1500 rpm; and the low-speed stirring speed described in S3 is ≤1000 rpm.

Citation Information

Patent Citations

  • Matte finishing varnish

    CN106883700A

  • High transparency matte finishing varnish and preparation method thereof

    CN107699076A

  • Interior wall water paint for children's bedroom and preparation method therefor

    WO2017016091A1