High-solid-content waterborne epoxy zinc-rich primer and preparation method thereof

The high-solid water-based epoxy zinc-rich primer addresses issues of incomplete wetting and high VOC by using modified resin and amine curing agents, enhancing adhesion and corrosion resistance, and reducing solvent use, resulting in improved storage stability and construction performance.

CN119081509APending Publication Date: 2024-12-06ZHEJIANG TIANNU GROUP PAINT MFG

Patent Information

Application Number
CN202411383766.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

Smart Images

  • Figure BDA0005070536910000021
    Figure BDA0005070536910000021
  • Figure BDA0005070536910000031
    Figure BDA0005070536910000031
  • Figure BDA0005070536910000032
    Figure BDA0005070536910000032
Patent Text Reader

Abstract

The invention belongs to the technical field of anticorrosive coatings, and particularly relates to a high-solid-content waterborne epoxy zinc-rich primer and a preparation method thereof. The invention aims to provide a high-solid-content waterborne epoxy zinc-rich primer with the advantages of high solid content, good constructability, long working life, good adhesive force, good water resistance, good salt fog resistance, stable storage and the like, and a preparation method of the high-solid-content waterborne epoxy zinc-rich primer, aiming at the defects of three existing waterborne epoxy zinc-rich primer systems. The paint comprises a component A, a component B and deionized water, the weight ratio of the component A to the component B is (8-10): 1; the deionized water accounts for 10-15% of the total weight; the paint has the characteristics that the content of non-volatile matters is more than or equal to 90% after the paint is prepared, the freeze-thaw stability is good, the early water resistance is good, the adhesive force is good, the VOC is less than 100g / L, the salt fog resistance is more than 1500h, and the paint does not rust, crack and bubble.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anticorrosive coatings, in particular to a high-solid water-based epoxy zinc-rich primer and a preparation method thereof. Background Art

[0002] Epoxy zinc-rich primer is a special coating mainly used in marine engineering, ships, storage tanks, steel structures, containers, petrochemical systems and other fields. It usually uses epoxy resin and zinc powder as the main raw materials. It has fast natural drying and strong adhesion, and the zinc powder provides anti-corrosion effect for the coating. Due to the high activity of zinc powder, in order to maintain long-term storage stability, the zinc powder component cannot contain water. There are three types of existing water-based epoxy zinc-rich primers: one is a three-component system consisting of a water-based epoxy emulsion component, a water-based epoxy curing agent component and a zinc powder component. The disadvantage is that the on-site mixed zinc powder is not thoroughly wetted, and bubbles are easily generated, resulting in incomplete protection of the steel and hidden dangers. The second is to use an epoxy curing agent containing a hydrophilic group but no water as a carrier of zinc powder, with other pigments, fillers, additives, etc. as the main agent, and epoxy emulsion as another component. The disadvantage is that a small amount of curing agent resin is used to coat the zinc powder, which requires a large amount of solvent dilution, resulting in high VOC, and the zinc powder is carried by a strong alkaline curing agent, which is not conducive to long-term storage stability. The third type is to use modified epoxy resin coated zinc powder as the main agent, with water-based epoxy curing agent. The disadvantage is that the application period is short and cannot meet the construction application. Since a large number of hydrophilic groups are introduced when modifying the epoxy resin, the anti-corrosion performance is poor. At the same time, compared with solvent-based zinc-rich primers, these three water-based zinc-rich primers have the disadvantages of poor substrate adhesion, low solid content, and poor construction performance.

[0003] Patent CN 113881317 A "A water-based epoxy zinc-rich primer and its preparation method and application" describes a water-based epoxy zinc-rich primer. Component A uses a modified bisphenol A epoxy resin emulsion with low reactivity, which effectively prolongs the reaction time after the A and B components are mixed, solving the problem of the short service life of ordinary water-based epoxy zinc-rich primers, which can be as long as 16 hours; at the same time, the modified bisphenol A epoxy resin emulsion has a high film-forming temperature and has the characteristics of fast drying of the paint film of a single-component coating, which can effectively prevent the adhesion of the paint film caused by the stacking of the plates; component B uses a water-soluble modified amine curing agent and other raw materials such as zinc powder to form a high-solid water-free component B with a solid content of more than 93%, which is combined with component A to effectively reduce the VOC content in the product, and the VOC content is below 200g / L. Water is used as a diluent during construction, which effectively reduces the emission of organic solvents and solves the problem of large environmental pollution of solvent-based epoxy zinc-rich primers. Patent CN 109912781A discloses a water-based epoxy curing agent for water-based epoxy resin, a preparation method and a use method thereof, and the obtained epoxy curing system has a fast curing speed and improved impact resistance. However, it contains a large number of amide bonds, which leads to strong hygroscopicity of the material after film formation and curing, and a significant decrease in water resistance and acid and alkali resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a high-solid water-based epoxy zinc-rich primer and a preparation method thereof, which has the advantages of high solid content, good workability, long application period, good adhesion, good water resistance, good salt spray resistance, storage stability, etc., in view of the shortcomings of the three existing water-based epoxy zinc-rich primer systems.

[0005] A high-solid water-based epoxy zinc-rich primer comprises a component A, a component B and deionized water; the weight ratio of the component A to the component B is 8-10:1; and the deionized water accounts for 10-15% of the total weight.

[0006] The component A comprises the following components in parts by weight, with a total amount of 100 parts:

[0007]

[0008]

[0009] The B component includes the following components in parts by weight, with a total amount of 100 parts:

[0010]

[0011] Preferably, the dispersant is a high molecular block copolymer with pigment affinity groups;

[0012] Preferably, the active diluent is a diepoxy-based ethylene glycol diglycidyl ether active diluent;

[0013] Preferably, the zinc powder is a mixture of flaky zinc powder and spherical zinc powder in a ratio of 1:10;

[0014] Preferably, the cosolvent is one or more of propylene glycol methyl ether, ethylene glycol tert-butyl ether, and ethylene glycol butyl ether;

[0015] Preferably, the carbon nanotube dispersion is a dispersion having a carbon nanotube content of 12%-14%;

[0016] Preferably, the filler is one or more of feldspar powder, silica powder, and barium sulfate;

[0017] Preferably, the silane coupling agent is an epoxy silane coupling agent containing reactive glycidoxy and methoxy groups;

[0018] Preferably, the anti-settling agent is one or more of fumed silica, bentonite powder, and attapulgite;

[0019] Preferably, the flash rust inhibitor is a flash rust inhibitor that does not contain nitrite;

[0020] The modified epoxy resin is prepared by the following method:

[0021] 65-70 parts of bisphenol A epoxy resin and 5-10 parts of epoxy-terminated hyperbranched polyester are put into a reaction kettle, the temperature is raised to 120±5°C, 15-20 parts of a mixed solution consisting of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and 8-10 parts of propylene glycol butyl ether are dripped in 0.5-1 hour, the temperature is reduced after keeping the temperature for 3-5 hours, and the modified epoxy resin with a solid content of ≥90% is synthesized and prepared; the total amount of each substance involved in the reaction is 100 parts.

[0022] Preferably, the bisphenol A epoxy resin is one of E-20, E-14 and E-12.

[0023] The above-mentioned water-based epoxy curing agent is prepared by the following method:

[0024] 23-33 parts of polyetheramine and 10-20 parts of polyethylene glycol diglycidyl ether are dissolved in 10-15 parts of propylene glycol butyl ether, the temperature is raised to 70±5°C, 15-20 parts of E20 epoxy resin are added and the temperature is kept for 2 hours; then a mixture consisting of 22-28 parts of meta-phenylenediamine and 5-10 parts of propylene glycol butyl ether is added, and the temperature is kept for 2-3 hours to obtain the water-based epoxy curing agent with a solid content of ≥80% and an active hydrogen equivalent of 130-150, and the total amount of the above materials participating in the reaction is 100 parts.

[0025] Preferably, the polyetheramine is one of D-230, M-3085 and M-2070;

[0026] Preferably, the molecular weight of the polyethylene glycol diglycidyl ether is one or more in the range of 1000-6000;

[0027] The modified corrosion inhibitor described above is prepared by the following method:

[0028] Weigh 1-2 parts of ZnNiAl-LDH and add them to 25-50 parts of deionized water and 25-50 parts of ethanol. After stirring evenly, add 0.3-1 parts of Na2MoO4·2H2O, adjust the pH to 9.5-10 with ammonia water, stir magnetically for 24 hours at a water bath temperature of (30±5)°C, wash with deionized water and ethanol until neutral, add 5-10 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol after drying, react at an oil bath temperature of 130°C±10°C for 10-12 hours, add 15-20 parts of ethanol and ultrasonicate for 1 hour, wash the residue with deionized water and ethanol, and obtain the modified corrosion inhibitor after drying; the total amount of various materials during synthesis is 100 parts.

[0029] Preferably, the ZnNiAl-LDH is a two-dimensional layered metal hydroxide from Xianfeng Nano;

[0030] Preparation of component A: Add modified epoxy resin, dispersant, active diluent and cosolvent into a batching pot, stir at a speed of (400-600) rpm for (5-10) minutes; then add filler, zinc powder and anti-settling agent in turn, adjust the stirring speed to (1000-1200) rpm, stir and disperse for (20-30) minutes, disperse to a fineness of ≤60μm and a temperature of ≤60°C; then add carbon nano dispersion and silane coupling agent in turn, rotate at a speed of (400-600) rpm, stir for (5-10) minutes, and mix evenly to obtain component A.

[0031] The core of the invention is to use O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol to improve the compatibility of epoxy resin and terminal epoxy hyperbranched polyester with cosolvent and water, reduce the amount of cosolvent used, and have certain hydrophobicity. Zinc powder can be coated after paint making, so as to avoid the reaction of zinc powder and water after large-area contact, and prolong the application period. The terminal epoxy hyperbranched polyester is used for toughening modification, and because it has multiple epoxy groups, it provides sufficient crosslinking and curing groups for the paint film, ensures the crosslinking density, and improves the initial water resistance. The modified m-phenylenediamine is modified by using polyetheramine, polyethylene glycol diglycidyl ether and E-20 epoxy resin with good hydrophilicity. The modified amine curing agent has moderate activity and can make the curing reaction proceed gently. The molecular chain segment of E20 epoxy resin is introduced to improve the compatibility of the curing agent and epoxy resin. The curing agent is self-emulsified by using polyetheramine and polyethylene glycol diglycidyl ether, and its flexible carbon branched structure can rotate freely and is elastic, which reduces the glass transition temperature of the curing agent, and the curing agent has sufficient time and space to diffuse into the interior of the resin particles for a full curing reaction. Molybdate is used to intercalate the two-dimensional layered metal hydroxide of ZnNiAl-LDH to improve the anti-corrosion effect of the molybdate corrosion inhibitor, and the Lewis acid-base interaction between O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and ZnNiAl-LDH is used to modify the intercalation corrosion inhibitor to prevent the particles from agglomerating or settling in the coating system, further improving the anti-corrosion effect. The use of flaky zinc powder and spherical zinc powder in a ratio of 1:10 not only takes into account the cost, but also significantly improves the corrosion resistance of the coating. The addition of epoxy silane coupling agent, which contains reactive glycidyl and methoxy groups, can not only promote the adhesion of the coating to the substrate, but also make the arrangement between the zinc powders more compact, forming an anode zinc protective layer, and improving the corrosion resistance of the coating. Carbon nano dispersion has excellent conductivity and nano-size effect. In the coating, it can not only extend the path for corrosive media (water, oxygen, etc.) to enter the surface of the steel substrate, but also transfer electrons in the cathodic protection stage, improve the cathodic protection of zinc powder, and enhance the anti-corrosion performance of the paint film. At the same time, adding an appropriate amount of diepoxy-based ethylene glycol diglycidyl ether active diluent during paint making can not only reduce the viscosity of the system, further reduce the use of organic solvents, improve the wettability of the substrate and filler, but also participate in the reaction during the film formation of the coating to improve the toughness of the coating.

[0032] 1. The present invention modifies epoxy resin and adds terminal epoxy hyperbranched polyester to prepare a high-solid and low-viscosity modified epoxy resin. After forming a film with a curing agent, the crosslinking density is high and the impact resistance is good.

[0033] 2. The water-based amine curing agent prepared by the present invention has moderate reactivity and can be used for 5 hours after painting. The curing agent has sufficient time and space to diffuse into the interior of the resin particles for a full curing reaction, with a surface drying time of ≤1 hour and a real drying time of ≤16 hours.

[0034] 3. The modified corrosion inhibitor prepared by the present invention has good dispersibility in the coating, is not easy to agglomerate, and improves the anti-corrosion performance of the paint film.

[0035] 4. Component A mainly composed of modified epoxy resin and component B mainly composed of modified water-based amine curing agent are compounded in proportion and matched with active diluent, carbon nano dispersion and zinc powder. After painting, the non-volatile matter content is ≥90%, the freeze-thaw stability is good, the early water resistance is good, the adhesion is good, VOC <100g / L, the salt spray resistance is >1500h, and it does not rust, crack or blister. DETAILED DESCRIPTION

[0036] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation method, structure, characteristics and effects of the present invention are described in detail below in combination with the preferred embodiments.

[0037] Example 1

[0038] Preparation of modified epoxy resin: 68 parts of bisphenol epoxy resin and 5 parts of terminal epoxy hyperbranched polyester (EHBP) are put into a reaction kettle, heated to (120±5)°C, and a mixed liquid consisting of 18 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and 9 parts of propylene glycol butyl ether is added dropwise within (0.5-1) h. After keeping warm for (3-5) h, the temperature is lowered and the material is discharged to synthesize a modified epoxy resin with a solid content of 91%.

[0039] Preparation of water-based amine curing agent: 28 parts of polyether amine and 15 parts of polyethylene glycol diglycidyl ether are dissolved in 10 parts of propylene glycol butyl ether, the temperature is raised to (70±5)°C, 18 parts of E20 epoxy resin are added and kept warm for 2 hours; then a mixture of 23 parts of meta-phenylenediamine and 6 parts of propylene glycol butyl ether is added, and the temperature is kept warm for (2-3) hours to obtain a water-based epoxy curing agent with a solid content of 84% and an active hydrogen equivalent of 147.

[0040] Preparation of modified corrosion inhibitor: Weigh 1.5 parts of ZnNiAl-LDH and add it to 38 parts of deionized water and 38 parts of ethanol. After stirring evenly, add 0.5 parts of Na2MoO4·2H2O, adjust the pH to 9.5-10 with ammonia water, stir magnetically for 24 hours at a water bath temperature of (30±5)℃, wash with deionized water and ethanol until neutral, add 7 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl)polypropylene glycol after drying, react at an oil bath temperature of (130±10)℃ for (10-12) hours, add 15 parts of ethanol and ultrasonicate for 1 hour, wash the residue with deionized water and ethanol, and obtain the modified corrosion inhibitor after drying.

[0041] Preparation of component A: 15 parts of modified epoxy resin, 0.3 parts of dispersant, 5 parts of active diluent, and 5 parts of cosolvent are added to a batching pot, and stirred at a speed of (400-600) rpm for (5-10 minutes); then 8 parts of filler, 65 parts of zinc powder, and 1 part of anti-settling agent are added in sequence, the stirring speed is adjusted to (1000-1200) rpm, and stirred and dispersed for (20-30) minutes until the fineness is ≤60μm and the temperature is ≤60°C; then 0.2 parts of carbon nano dispersion and 0.5 parts of silane coupling agent are added in sequence, the speed is (400-600) rpm, stirred for (5-10) minutes, and mixed evenly to obtain component A.

[0042] Preparation of component B: put 85 parts of waterborne epoxy curing agent into a batching pot, add 5 parts of anti-flash rust agent and 2 parts of modified corrosion inhibitor while stirring at a speed of (400-600) rpm, add 8 parts of deionized water after stirring evenly, stir for (10-15) minutes to mix evenly to obtain component B.

[0043] Preparation of primer: Add component B to component A and stir manually for (3-5) minutes until completely emulsified to obtain waterborne epoxy zinc-rich primer. Add deionized water to adjust the spraying viscosity and spray the sample to test the performance. The mass ratio of component A to component B is 8-10:1.

[0044] Example 2

[0045] Preparation of modified epoxy resin: 65 parts of bisphenol epoxy resin and 10 parts of terminal epoxy hyperbranched polyester (EHBP) are put into a reaction kettle, heated to (120±5)°C, and a mixed liquid consisting of 17 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and 8 parts of propylene glycol butyl ether is added dropwise within (0.5-1) h. After keeping warm for (3-5) h, the temperature is lowered and the material is discharged to synthesize a modified epoxy resin with a solid content of 92%.

[0046] Preparation of water-based amine curing agent: 23 parts of polyether amine and 18 parts of polyethylene glycol diglycidyl ether are dissolved in 11 parts of propylene glycol butyl ether, the temperature is raised to (70±5)°C, 18 parts of E20 epoxy resin are added and kept warm for 2 hours; then a mixture of 25 parts of meta-phenylenediamine and 5 parts of propylene glycol butyl ether is added, and the temperature is kept warm for (2-3) hours to obtain a water-based epoxy curing agent with a solid content of 80% and an active hydrogen equivalent of 143.

[0047] Preparation of modified corrosion inhibitor: Weigh 2 parts of ZnNiAl-LDH and add them to 31 parts of deionized water and 45 parts of ethanol. After stirring evenly, add 0.8 parts of Na2MoO4·2H2O, adjust the pH to 9.5-10 with ammonia water, stir magnetically for 24 hours at a water bath temperature of (30±5)℃, wash with deionized water and ethanol until neutral, add 6.2 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl)polypropylene glycol after drying, react at an oil bath temperature of (130±10)℃ for (10-12) hours, add 15 parts of ethanol and ultrasonicate for 1 hour, wash the residue with deionized water and ethanol, and obtain the modified corrosion inhibitor after drying.

[0048] Preparation of component A: 10.2 parts of modified epoxy resin, 0.2 parts of dispersant, 5 parts of active diluent, and 4.9 parts of cosolvent are added to a batching pot, and stirred at a speed of (400-600) rpm for (5-10 minutes); then 8 parts of filler, 70 parts of zinc powder, and 1 part of anti-settling agent are added in sequence, the stirring speed is adjusted to (1000-1200) rpm, and stirred and dispersed for (20-30) minutes until the fineness is ≤60μm and the temperature is ≤60°C; then 0.2 parts of carbon nano dispersion and 0.5 parts of silane coupling agent are added in sequence, the speed is (400-600) rpm, stirred for (5-10) minutes, and mixed evenly to obtain component A.

[0049] Preparation of component B: put 89 parts of waterborne epoxy curing agent into a batching pot, add 3 parts of anti-flash rust agent and 0.5 parts of modified corrosion inhibitor while stirring at a speed of 400-600 rpm, add 8 parts of deionized water after stirring evenly, stir for (10-15) minutes to mix evenly to obtain component B.

[0050] Preparation of primer: Add component B to component A and stir manually for (3-5) minutes until completely emulsified to obtain waterborne epoxy zinc-rich primer. Add appropriate amount of deionized water to adjust to spray viscosity and spray on the sample to test performance. The mass ratio of component A to component B is 8-10:1.

[0051] Example 3

[0052] Preparation of modified epoxy resin: 70 parts of bisphenol epoxy resin and 5 parts of terminal epoxy hyperbranched polyester (EHBP) are put into a reaction kettle, heated to (120±5)°C, and a mixed liquid consisting of 17 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and 8 parts of propylene glycol butyl ether is added dropwise within (0.5-1) h. After keeping warm for (3-5) h, the temperature is lowered and the material is discharged to synthesize a modified epoxy resin with a solid content of 92%.

[0053] Preparation of water-based amine curing agent: 33 parts of polyether amine and 15 parts of polyethylene glycol diglycidyl ether are dissolved in 10 parts of propylene glycol butyl ether, the temperature is raised to (70±5)°C, 15 parts of E20 epoxy resin are added and kept warm for 2 hours; then a mixture of 22 parts of meta-phenylenediamine and 5 parts of propylene glycol butyl ether is added, and the temperature is kept warm for (2-3) hours to obtain a water-based epoxy curing agent with a solid content of 85% and an active hydrogen equivalent of 138.

[0054] Preparation of modified corrosion inhibitor: Weigh 1 part of ZnNiAl-LDH and add it to 25 parts of deionized water and 43 parts of ethanol. After stirring evenly, add 1 part of Na2MoO4·2H2O, adjust the pH to 9.5-10 with ammonia water, stir magnetically for 24 hours at a water bath temperature of (30±5)℃, wash with deionized water and ethanol until neutral, add 10 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl)polypropylene glycol after drying, react at an oil bath temperature of (130±10)℃ for (10-12) hours, add 20 parts of ethanol and ultrasonicate for 1 hour, wash the residue with deionized water and ethanol, and obtain the modified corrosion inhibitor after drying.

[0055] Preparation of component A: 15 parts of modified waterborne epoxy resin, 0.3 parts of dispersant, 3 parts of active diluent, and 3 parts of cosolvent are added to a batching pot, and stirred at a speed of (400-600) rpm for (5-10) minutes; then 2 parts of filler, 75 parts of zinc powder, and 1 part of anti-settling agent are added in sequence, the stirring speed is adjusted to (1000-1200) rpm, and stirred and dispersed for (20-30) minutes until the fineness is ≤60μm and the temperature is ≤60°C; then 0.3 parts of carbon nano dispersion and 0.4 parts of silane coupling agent are added in sequence, the speed is (400-600) rpm, stirred for (5-10) minutes, and mixed evenly to obtain component A.

[0056] Preparation of component B: put 80 parts of waterborne epoxy curing agent into a batching pot, add 5 parts of anti-flash rust agent and 3 parts of modified corrosion inhibitor while stirring at a speed of (400-600) rpm, stir evenly, then add 10 parts of deionized water, stir for (10-15) minutes to mix evenly to obtain component B.

[0057] Preparation of primer: Add component B to component A and stir manually for (3-5) minutes until completely emulsified to obtain waterborne epoxy zinc-rich primer. Add appropriate amount of deionized water to adjust to spray viscosity and spray on the sample to test performance. The mass ratio of component A to component B is 8-10:1.

[0058] The test results are compared with the industry standard HG / T 3668-2020 "Zinc-rich Primer" as follows.

[0059]

[0060]

Claims

1. A high solid waterborne epoxy zinc-rich primer, characterized in that: It includes component A, component B and deionized water; the deionized water accounts for 10-15% of the total weight; the weight ratio of component A to component B is 8-10:1; The component A comprises the following components in parts by weight, with a total amount of 100 parts: The B component includes the following components in parts by weight, with a total amount of 100 parts:

2. The method for preparing the above-mentioned high-solid water-based epoxy zinc-rich primer is characterized in that: Preparation of component A: add modified epoxy resin, dispersant, active diluent and cosolvent into a batching pot, stir at a speed of 400-600rpm for 5-10 minutes; then add filler, zinc powder and anti-settling agent in turn, adjust the stirring speed to 1000-1200rpm, stir and disperse for (20-30) minutes, disperse to a fineness of ≤60μm, and a temperature of ≤60°C; then add carbon nano dispersion and silane coupling agent in turn, at a speed of 400-600rpm, stir for (5-10) minutes, and mix evenly to obtain component A; add component B The materials are prepared according to the proportions, the water-based epoxy curing agent is put into the batching pot, the anti-flash rust agent and the modified corrosion inhibitor are added under stirring at a speed of 400-600rpm, deionized water is added after stirring evenly, and the mixture is stirred for 10-15 minutes to obtain component B; component B is added to component A and stirred manually for 3-5 minutes until it is completely emulsified to obtain a water-based epoxy zinc-rich primer, deionized water is added, and the mass ratio of component A to component B is 8-10:

1. At this time, the deionized water added is 15% of the total amount of component A, component B and deionized water.

3. A high solid waterborne epoxy zinc-rich primer, characterized in that: The modified epoxy resin is prepared by the following method: 65-70 parts of bisphenol A epoxy resin and 5-10 parts of epoxy-terminated hyperbranched polyester are put into a reaction kettle, the temperature is raised to 120±5° C., 15-20 parts of a mixed solution consisting of O-(2-aminopropyl)-O'-(2-methoxyethyl) polypropylene glycol and 8-10 parts of propylene glycol butyl ether are dripped in 0.5-1 hour, the mixture is kept warm for 3-5 hours, and then the temperature is lowered and the mixture is discharged to synthesize a modified epoxy resin having a solid content of ≥90%; The total amount of each substance involved in the reaction is 100 parts.

4. A high solid waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The waterborne epoxy curing agent is prepared by the following method: dissolving 23-33 parts of polyetheramine and 10-20 parts of polyethylene glycol diglycidyl ether in 10-15 parts of propylene glycol butyl ether, heating to 70±5°C, adding 15-20 parts of E20 epoxy resin and keeping warm for 2 hours; then adding a mixture consisting of 22-28 parts of meta-phenylenediamine and 5-10 parts of propylene glycol butyl ether, keeping warm for 2-3 hours, and obtaining the waterborne epoxy curing agent with a solid content of ≥90% and an active hydrogen equivalent of 130-150, and the total amount of the above materials participating in the reaction is 100 parts.

5. A high solid waterborne epoxy zinc-rich primer according to claim 1, characterized in that: The modified corrosion inhibitor described above is prepared by the following method: weigh 1-2 parts of ZnNiAl-LDH, add them to 25-50 parts of deionized water and 25-50 parts of ethanol, stir evenly, add 0.3-1 parts of Na2MoO4·2H2O, adjust the pH to 9.5-10 with ammonia water, stir magnetically for 24 hours at a water bath temperature of (30±5)°C, wash with deionized water and ethanol until neutral, add 5-10 parts of O-(2-aminopropyl)-O'-(2-methoxyethyl)polypropylene glycol after drying, react at an oil bath temperature of 130°C±10°C for 10-12 hours, add 15-20 parts of ethanol and ultrasonicate for 1 hour, wash the residue with deionized water and ethanol, and obtain the modified corrosion inhibitor after drying; the total amount of various materials during synthesis is 100 parts.

Citation Information

Patent Citations

  • Epoxy curing agent

    CN109912781A

  • Waterborne epoxy zinc-rich primer as well as preparation method and application thereof

    CN113881317A

  • Waterborne epoxy zinc-rich paint modified by nanometer conductive carbon material and preparation method thereof

    CN103497636A

  • VOC (Volatile Organic Compounds)-free water-based epoxy curing agent

    CN103788343A

  • Low-VOC (volatile organic compound) water-based bi-component epoxy zinc-rich coating and preparation method thereof

    CN114106608A

Cited By

  • Epoxy zinc-rich primer for offshore photovoltaic bracket and preparation method of epoxy zinc-rich primer

    CN122521201A

  • Epoxy zinc-rich primer for offshore photovoltaic support and preparation method thereof

    CN122521201B