Two-component high-hardness scratch-resistant automobile finishing protective varnish and preparation method thereof
Through the preparation of two-component high-hard scratch-resistant car cover photoprotection varnish, the use of hydroxyacrylic resin, polyester polyol and isocyanate, the problem of softening and poor scratch resistance of existing car cover photoprotection coatings at high temperatures is solved. , realizes rapid drying and curing and high hardness coatings, significantly improving scratch and wear resistance.
Patent Information
- Application Number
- CN202411148008.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-06
AI Technical Summary
The existing automotive cover photoprotection coatings soften at high temperatures, have poor scratch resistance, and are not highly protective to the next coating, making it difficult to meet the needs of rapid drying, curing and high hardness.
Two-component high hardness scratch-resistant car cover photoprotection varnish is adopted, including 50 to 60 parts of hydroxyacrylic resin, 3 to 5 parts of polyester polyol, 1 to 1.5 parts of silicone scratch-resistant wax pulp, 20 to 25 parts of isocyanate, 0.5 to 1 part of polymer dispersant and 0.5 to 1 part of leveling agent are prepared by high-speed mixing and grinding, and the viscosity is controlled between 1000 to 1200mPa·s. Two-component AB is combined at a weight ratio of 4:1, and cured at room temperature for 24 The pencil hardness reaches 3H or more in hours, and the hardness can reach 4H or more after baking at 75℃.
A high-hardness coating that quickly cures at room temperature has been achieved, with significantly improved scratch resistance and wear resistance. The hardness of the coating film reaches pencil hardness above 4H, and the wear loss that meets GB/T 9286-1998 standards is 0.012g, long-term Resistant to scratches and wear.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention discloses a two-component high-hardness scratch-resistant automobile finishing protective varnish and a preparation method thereof, belonging to the field of automobile repair coatings. Background Art
[0002] With the improvement of people's living standards, the number of domestic household cars has continued to increase. The care and maintenance of cars in daily life have created higher demands for car coatings. In addition, due to the need for some repairs, it is often necessary to prepare a full, transparent, high-hardness, scratch-resistant protective coating.
[0003] At present, automobile coatings contain relatively high levels of organic solvents. The automobile repair market develops automobile coatings with single-component materials. The coatings are prone to powdering and fading due to long-term exposure to sunlight and rain, and have poor temperature resistance. At high temperatures, the coating softens, resulting in insufficient hardness and poor scratch resistance, and poor protection for the next coating. Two-component automobile finishing and repair varnishes must be heated to a certain temperature or treated in other ways to achieve the required hardness and weather resistance. Generally, the paint film is still relatively soft, has poor scratch resistance, is not resistant to alternating hot and cold temperatures, and has weak protection for the underlying coating film. Therefore, it is the primary task in the field of research and development technology to develop a two-component automobile finishing varnish with fast drying and curing, high coating hardness, and scratch resistance as soon as possible. Summary of the invention
[0004] In view of the shortcomings of the existing protective layer automobile finishing technology, the purpose of the present invention is to provide a two-component high-hardness scratch-resistant automobile finishing protective varnish and a preparation method thereof to solve the problem.
[0005] In order to achieve the above-mentioned purpose, the present invention is realized through the following technical scheme: comprising the following raw materials in parts by weight: 50 to 60 parts of hydroxy acrylic resin, 3 to 5 parts of polyester polyol, 1 to 1.5 parts of silicone anti-scratch wax slurry, 20 to 25 parts of isocyanate, 16 to 18 parts of mixed solvent, 0.5 to 1 part of polymer dispersant and 0.5 to 1 part of leveling agent.
[0006] Preferably, the relative molecular mass of the hydroxy acrylic resin is 2000-5000.
[0007] Preferably, the relative molecular mass of the polyester polyol is 1000-2000.
[0008] Preferably, the organosilicon anti-scratch wax slurry is in a viscous fluid state.
[0009] Preferably, the mixed solvent is a mixture of PMA, xylene and butyl acetate in a weight ratio of 5:3:2.
[0010] A method for preparing a two-component high-hardness scratch-resistant automobile varnish, comprising the following steps:
[0011] Step 1: Prepare a first mixed stock solution, and mix the polyester polyol, dispersant and silicone anti-scratch wax slurry at high speed;
[0012] Step 2: Prepare a second mixed stock solution, grind the first mixed stock solution until the mixed raw material is ground to a fineness of less than 15 um;
[0013] Step 3: prepare a third mixed stock solution, and mix the hydroxy acrylic resin and the defoaming and leveling additive at a high speed;
[0014] Step 4: Prepare a fourth mixed stock solution, and slowly add the second mixed stock solution to the dispersed third mixed stock solution;
[0015] Step 5: Adjust the viscosity by gradually adding the mixed solvent to the fourth mixed stock solution and measuring the viscosity in real time to obtain varnish component A.
[0016] Step 6: Prepare the varnish B component by uniformly mixing the isocyanate resin and the fourth mixed stock solution in a weight ratio of 3:1.
[0017] Preferably, the polyester polyol added in step 1 accounts for 70-80% of the total amount; and the rotation speed is maintained at at least 1800 r / min, and the high-speed dispersion time is at least 30 min.
[0018] Preferably, in step 1, the organosilicon anti-scratch wax slurry is pretreated by the following steps:
[0019] S1; grinding the silicone anti-scratch wax slurry after wetting it with a dispersant;
[0020] S2: Cool and pack for standby use, and add and mix after the third mixed stock solution is completed.
[0021] Preferably, in step 5, when adjusting the viscosity, the temperature is stabilized at 24-26°C.
[0022] Preferably, in step 5, the viscosity is controlled within a range of 1000 to 1200 mPa·s.
[0023] Beneficial Effects
[0024] The present invention selects low molecular weight hydroxy acrylic resin as the main film-forming substance and combines it with high hardness polyester polyol and isocyanate for high cross-linking, and adds anti-scratch wax slurry without affecting the transparency of the coating film to prepare a spray-type, high hardness, scratch-resistant automobile finishing protective varnish, which solves the problems of insufficient finishing hardness during the current automobile repair paint construction, the need for baking and curing, high requirements for the construction environment, and poor scratch resistance after film formation.
[0025] The coating of the present invention is constructed after compounding AB two components at a weight ratio of 4:1. The hardness of the pencil can reach above 3H after curing at room temperature for 24 hours, and the hardness can reach above 4H after baking at 75°C for 40 minutes. In addition, under the GB / T 9286-1998 standard, the coating is tested for a wear loss of 0.012g at 750g / 1000r. It can be concluded that the two-component high-hardness scratch-resistant automobile varnish can resist scratches and wear for a long time, and the coating hardness performance is good. DETAILED DESCRIPTION
[0026] In order to make the technical research and development means, creative thinking characteristics, and performance objectives achieved by the present invention easy to understand and comprehend, the present invention is further described below in conjunction with specific implementation methods.
[0027] The present invention provides a one-component high-temperature resistant heat-insulating coating technical solution: comprising the following raw materials in parts by weight: comprising the following raw materials in parts by weight: 50 to 60 parts of hydroxy acrylic resin, 3 to 5 parts of polyester polyol, 1 to 1.5 parts of silicone anti-scratch wax slurry, 20 to 25 parts of isocyanate, 16 to 18 parts of mixed solvent, 0.5 to 1 part of polymer dispersant and 0.5 to 1 part of leveling agent.
[0028] Preferably, the relative molecular mass of the hydroxy acrylic resin is 2000-5000.
[0029] Preferably, the relative molecular mass of the polyester polyol is 1000-2000.
[0030] Preferably, the organosilicon anti-scratch wax slurry is in a viscous fluid state.
[0031] Preferably, the mixed solvent is a mixture of PMA, xylene and butyl acetate in a weight ratio of 5:3:2.
[0032] A method for preparing a two-component high-hardness scratch-resistant automobile varnish, comprising the following steps:
[0033] Step 1: Prepare a first mixed stock solution, and mix the polyester polyol, dispersant and silicone anti-scratch wax slurry at high speed;
[0034] Step 2: Prepare a second mixed stock solution, grind the first mixed stock solution until the mixed raw material is ground to a fineness of less than 15 um;
[0035] Step 3: prepare a third mixed stock solution, and mix the hydroxy acrylic resin and the defoaming and leveling additive at a high speed;
[0036] Step 4: Prepare a fourth mixed stock solution, and slowly add the second mixed stock solution to the dispersed third mixed stock solution;
[0037] Step 5: Adjust the viscosity by gradually adding the mixed solvent to the fourth mixed stock solution and measuring the viscosity in real time to obtain varnish component A.
[0038] Step 6: Prepare the varnish B component by uniformly mixing the isocyanate resin and the fourth mixed stock solution in a weight ratio of 3:1.
[0039] Preferably, the polyester polyol added in step 1 accounts for 70-80% of the total amount; and the rotation speed is maintained at at least 1800 r / min, and the high-speed dispersion time is at least 30 min.
[0040] Preferably, in step 1, the organosilicon anti-scratch wax slurry is pretreated by the following steps:
[0041] S1; grinding the silicone anti-scratch wax slurry after wetting it with a dispersant;
[0042] S2: Cool and pack for standby use, and add and mix after the third mixed stock solution is completed.
[0043] Preferably, in step 5, when adjusting the viscosity, the temperature is stabilized at 24-26°C.
[0044] Preferably, in step 5, the viscosity is controlled within a range of 1000 to 1200 mPa·s.
[0045] Example 1
[0046] The silicone anti-scratch wax slurry is pretreated by the following steps;
[0047] S1: grinding the silicone anti-scratch wax slurry after dispersant wetting treatment, the grinding time is 10min;
[0048] S2: Cool and pack for standby use, and add and mix other materials after they are prepared.
[0049] A two-component high-hardness scratch-resistant automobile varnish is prepared by the following steps:
[0050] Step 1, prepare a first mixed stock solution, mix 5 parts of polyester polyol, 0.5 parts of dispersant and 1.5 parts of silicone anti-scratch wax slurry, increase the speed of the disperser to 1800r / min and perform high-speed dispersion for 30 minutes;
[0051] Step 2, grinding the mixed raw materials and regularly testing the grinding fineness until the mixed raw materials are ground to a fineness less than 15 um, thereby obtaining a second mixed stock solution;
[0052] Step 3, 60 parts of hydroxy acrylic resin and 1 part of defoaming and leveling agent are mixed, and the speed of the disperser is increased to 1800 r / min for high-speed dispersion for 30 minutes to obtain a third mixed stock solution;
[0053] Step 4: prepare a fourth mixed stock solution, slowly add 7 parts of the second mixed stock solution to 61 parts of the third mixed stock solution being dispersed, and maintain high-speed dispersion for 10 minutes;
[0054] Step 5: Use 12 parts of mixed solvent to adjust the viscosity. The mixed solvent is gradually added to the fourth mixed stock solution prepared in step 4, and the viscosity is measured in real time until it reaches 1100 mPa·s to prepare varnish A component.
[0055] Step 6: Mix 15 parts of isocyanate resin and 5 parts of mixed solvent in a weight ratio of 3:1 to obtain varnish component B.
[0056] The hydroxyl acrylic resin adopts FS-3070 hydroxyl acrylic resin with a solid content of >70% from Haimingsteqian Co., Ltd. and a relative molecular mass of 3000-3500; the polyester polyol adopts 100% solid polyol from Haimingsteqian Co., Ltd., the silicone anti-scratch wax slurry adopts DC-18 from Dow Corning, and the isocyanate resin adopts HI-100 isocyanate trimer from BASF, with a parameter of NCO=22%, and has excellent flexibility, corrosion resistance, temperature resistance and tensile resistance.
[0057] After the varnish component A is mixed with the varnish component B, the product spray construction performance indicators are shown in Table 1.
[0058] Example 2
[0059] The difference from Example 1 is that the added 60 parts of hydroxy acrylic resin is FS-2970A resin with a relative molecular weight of 3500-4500.
[0060] The hydroxy acrylic resin adopts FS-2970A hydroxy acrylic resin with a solid content of more than 70% produced by Haimingsdeqian Co., Ltd.
[0061] The product spraying construction performance indicators are shown in Table 1.
[0062] Example 3
[0063] The difference from Example 1 is that the 60 parts of hydroxyl acrylic resin added are replaced by a mixture of 33 parts of hydroxyl acrylic resin FS-4470 and 27 parts of hydroxyl acrylic resin FS-2970A.
[0064] The hydroxy acrylic resins used are FS-4470 hydroxy acrylic resin with a relative molecular mass of 2500-3000 and a solid content of more than 70% and FS-2970 hydroxy acrylic resin with a relative molecular mass of 3500-4500 and a solid content of more than 70% from Haimingsdeqian Co., Ltd.
[0065] The product spraying construction performance indicators are shown in Table 1.
[0066] Table 1
[0067]
[0068] As shown in Table 1, the two-component high-hardness scratch-resistant automobile varnish prepared in Examples 1 to 3 can reach a hardness of 3H or more after curing at room temperature for 24 hours. After baking at 80°C for 1 hour, the hardness can reach 4H or more. And under the GB / T9286-1998 standard, the wear loss of the coating tested is less than 0.03g.
[0069] As shown in Table 1, based on the adjustment of the molecular weight of the hydroxyl acrylic resin in Example 1-Example 2, it can be concluded that the relative molecular weight of the added hydroxyl acrylic resin affects the hardness of the finished product. The larger the molecular weight of the hydroxyl acrylic resin, the higher its viscosity, and the higher its wear resistance and coating gloss.
[0070] Based on the adjustment of the weight percentage of the resin blend in Example 1 and Example 3, it was found that although the mixed hydroxy acrylic resin met the test standard, the gloss of the coating film was lower than that of the hydroxy acrylic resin in Example 1, which means that the FS-4470 hydroxy acrylic resin and the FS-2970 hydroxy acrylic resin interacted with each other when mixed. This intermolecular interaction led to a decrease in glossiness, but improved wear resistance. Therefore, it can be concluded that under a certain budget, hydroxy acrylic resins can be mixed to formulate car bodies with different requirements.
[0071] Comparative Example 1
[0072] The difference from Example 1 is that the added 60 parts of hydroxy acrylic resin has a relative molecular mass greater than 5000.
[0073] Comparative Example 2
[0074] The difference from Example 1 is that the added 60 parts of hydroxy acrylic resin has a relative molecular mass of less than 2000.
[0075] After testing, in Comparative Examples 1-2, hydroxy acrylic resin and isocyanate resin are the main film-forming substances of the coating, which have high weather resistance and UV resistance and good cross-linking and curing film-forming properties, but the hydroxy acrylic resin with too high relative molecular weight has poor flow and leveling properties, making it difficult for the spray paint to flow naturally and cover the car body. The hydroxy acrylic resin with too low relative molecular weight has poor curing properties, making it difficult for the spray paint to flow on the car body; therefore, the selection range of the relative molecular weight of the hydroxy acrylic resin is 2000-5000, which helps to ensure the high solid content and flow and leveling properties of the coating, and ensures that the coating film is plump and thick.
[0076] Comparative Example 3
[0077] The difference from Example 1 is that the added 5 parts of polyester polyol is changed to 7 parts.
[0078] After testing, in comparative example 3, polyester polyol is a high cross-linking reaction promoting material with drying and cross-linking curing properties. Its main function is to reduce the viscosity of the coating, and it participates in the film-forming reaction to further improve the fullness of the coating. At the same time, it also promotes the reaction process of the main material, so that it can be solid in the coating, effectively achieving high hardness and scratch resistance, thereby improving the scratch resistance of the coating. After adding 7 parts of polyester polyol, it was found that the viscosity of the varnish was too low, and more curing agent (hydroxy acrylic resin) needed to be added in step 5 to meet the condition of viscosity reaching 1100mPa·s. Therefore, based on cost considerations, choosing 3 to 5 parts of polyester polyol is the best.
[0079] The wear and scratch resistance of the coating is further improved by using polyester polyols and silicone anti-scratch wax slurry.
[0080] The addition amount of silicone anti-scratch wax slurry is between 1 and 1.5 parts. It mainly floats on the surface of the coating when the coating is formed into a film, which plays a role in reducing the surface friction coefficient and lowering the surface tension. The silicone anti-scratch wax slurry can be tightly combined with other components in the coating to form a floating plane structure, thereby improving the scratch resistance and wear resistance of the coating.
[0081] The selection of isocyanate resin, HDI trimer material with excellent UV resistance, is to ensure that the coating can maintain a stable color in harsh environments. It is compounded as the B component of the product, which not only provides weather resistance for the coating, but also improves the heat and impact resistance of the coating to a certain extent.
[0082] The mixed solvent includes PMA, xylene and butyl acetate, and its main function is to serve as a solvent and diluent for the coating. The addition of the mixed solvent helps to adjust the viscosity and fluidity of the coating, so that the coating can better wet and disperse the pigments and fillers during the construction process, and improve the construction performance and storage stability of the coating.
[0083] Finally, the addition amount of polymer dispersant and defoaming and leveling agent is 0.5-1 part each. The main function of dispersant is to promote the dispersion of pigments and fillers and prevent them from agglomerating in the coating. Polymer dispersant can effectively reduce the surface tension of pigments and fillers, making them better dispersed in the coating and improving the uniformity and stability of the coating; the main function of defoaming and leveling agent is to promote the surface leveling of the coating during construction and eliminate coating defects caused by foam.
[0084] In summary, the basic principles of the coating composition and the main features of the coating of the present invention and the advantages of the present invention are shown and described above. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any mark in the claims should not be regarded as limiting the claims involved.
[0085] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A two-component high-hardness scratch-resistant automotive varnish protection varnish, Features: The invention comprises the following raw materials in parts by weight: 50-60 parts of hydroxy acrylic resin, 3-5 parts of polyester polyol, 1-1.5 parts of organosilicon anti-scratch wax slurry, 20-25 parts of isocyanate, 16-18 parts of mixed solvent, 0.5-1 part of polymer dispersant and 0.5-1 part of leveling agent.
2. A two-component high-hardness scratch-resistant automobile varnish protection varnish according to claim 1, Features: The relative molecular mass of the hydroxy acrylic resin is 2000-5000.
3. A two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: The relative molecular mass of the polyester polyol is 1000-2000.
4. A two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: The organosilicon anti-scratch wax slurry is in a viscous fluid state.
5. A two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: The mixed solvent is a mixture of PMA, xylene and butyl acetate in a weight ratio of 5:3:
2.
6. A method for preparing a two-component high-hardness scratch-resistant automobile varnish, Features The preparation comprises the following steps: Step 1; A first mixed stock solution is prepared by mixing the polyester polyol, the dispersant and the silicone anti-scratch wax slurry at a high speed; Step 2; Prepare a second mixed stock solution by grinding the first mixed stock solution until the mixed raw materials are ground to a fineness less than 15 um; Step 3; A third mixed stock solution is prepared by mixing the hydroxy acrylic resin and the defoaming and leveling agent at a high speed; Step 4: Prepare a fourth mixed stock solution, and slowly add the second mixed stock solution to the dispersed third mixed stock solution; Step 5: Adjust the viscosity by gradually adding the mixed solvent to the fourth mixed stock solution and measuring the viscosity in real time to obtain varnish component A. Step 6: Prepare the varnish B component by uniformly mixing the isocyanate resin and the fourth mixed stock solution in a weight ratio of 3:
1.
7. A method for preparing a two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: The polyester polyol added in step 1 accounts for 70-80% of the total amount; and the rotation speed is maintained at at least 1800r / min, and the high-speed dispersion time is at least 30min.
8. A method for preparing a two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: In step 1, the organosilicon anti-scratch wax slurry is pretreated by the following steps; S1; grinding the silicone anti-scratch wax slurry after wetting it with a dispersant; S2: Cool and pack for standby use, and add and mix after the third mixed stock solution is completed.
9. A method for preparing a two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: In step 5, when viscosity adjustment is performed, the temperature is stabilized at 24-26°C.
10. A method for preparing a two-component high-hardness scratch-resistant automobile varnish according to claim 1, Features: In step 5, the viscosity is controlled within a range of 1000 to 1200 mPa·s.
Citation Information
Patent Citations
Dual-component polyurethane paint composition comprising composition of isocyanurates derived from di(isocyanatomethyl)cyclohexane and aliphatic diisocyanate
CN102477251A
Quick-drying scratch-resistant varnish composition with high solid content as well as preparation method and application of quick-drying scratch-resistant varnish composition
CN105949983A
Automobile exterior trimming varnish meeting high orange peel requirement as well as preparation method and construction method of automobile exterior trimming varnish
CN114921167A
One-pack composition for automotive clearcoat with improved chemical resistance, scratch resistance and scratch recovery property
KR1020130078644A