Two-component waterborne polyurethane coating, preparation method thereof and coated product

By optimizing the composition distribution ratio and reaction treatment of two-component water-based polyurethane coatings, the cross-linking density and weather resistance of the coating are improved, and the problem of poor weather resistance of traditional coatings is solved, and better water resistance and salt spray resistance are achieved.

CN119081528APending Publication Date: 2024-12-06ZHANJIANG POWER SUPPLY BUREAU OF GUANGDONG POWER GRID CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411442820.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional two-component aqueous acrylic polyurethane coatings have poor weather resistance, which is mainly due to the low crosslinking density and excessive urea bond formation, which affects its weather resistance.

Method used

Two-component aqueous polyurethane coatings using specific component distribution ratios include components A and components B. Component A is composed of hydroxyacrylate, acrylic monomers and acrylic monomers with main carbon chains of 4 to 6 As functional monomers, the esters containing tertiary carbon structures and di-tertiary carbon isocyanurate are composed of isocyanate-based curing agents. Through polymerization and neutralizing agent treatment, the reaction selectivity of isocyanate-based curing agents is optimized. , reduce urea bond formation and improve crosslinking density.

Benefits of technology

It significantly improves the weather resistance, water resistance and salt spray resistance of two-component water-based polyurethane coatings, and extends the service life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention relates to a two-component waterborne polyurethane coating, a preparation method thereof and a coating product. The double-component waterborne polyurethane coating comprises a component A and a component B, the component A is prepared from the following components in parts by mass: 20 to 40 parts of hydroxyl acrylate, 1 to 8 parts of acrylic acid monomer, 30 to 50 parts of acrylic ester monomer, 10 to 40 parts of functional monomer, 0.05 to 5 parts of initiator, 0.05 to 5 parts of chain transfer agent, 1 to 10 parts of neutralizer, 30 to 100 parts of organic solvent and 30 to 500 parts of water; the functional monomers comprise a first monomer and a second monomer, the first monomer comprises ester containing a tertiary carbon structure and having a main carbon chain of 4-6 carbon atoms, and the second monomer comprises bis (tertiary carbon isocyanurate) glyceride; and the component B comprises an isocyanate curing agent. The two-component waterborne polyurethane coating has relatively good weather resistance, water resistance, salt mist resistance and aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and in particular to a two-component waterborne polyurethane coating and a preparation method thereof, and a coating product. Background Art

[0002] At present, two-component waterborne acrylic polyurethane coatings have important applications in the fields of power, rail transit, automobiles, high-end engineering machinery, flooring, wood products, etc., and are developing day by day. Two-component waterborne acrylic polyurethane coatings include two-component solvent-based acrylic polyurethane coatings and two-component waterborne acrylic polyurethane coatings. Two-component solvent-based acrylic polyurethane coatings have better weather resistance, while traditional two-component waterborne acrylic polyurethane coatings have poor weather resistance.

[0003] Therefore, it is necessary to improve the traditional technology. Summary of the invention

[0004] Based on this, the present application provides a two-component waterborne polyurethane coating with good weather resistance, a preparation method thereof, and a coating product.

[0005] The technical solution of this application to solve the above technical problems is as follows.

[0006] In a first aspect, the present application provides a two-component waterborne polyurethane coating, comprising component A and component B;

[0007] The component A comprises the following components by mass: 20-40 parts of hydroxy acrylate, 1-8 parts of acrylic monomer, 30-50 parts of acrylate monomer, 10-40 parts of functional monomer, 0.05-5 parts of initiator, 0.05-5 parts of chain transfer agent, 1-10 parts of neutralizer, 30-100 parts of organic solvent and 30-500 parts of water; the functional monomer comprises a first monomer and a second monomer, the first monomer comprises an ester containing a tertiary carbon structure with a main carbon chain of 4-6 carbon atoms, and the second monomer comprises di-tertiary carbon isocyanuric acid glyceryl ester;

[0008] The B component includes an isocyanate curing agent.

[0009] In some of the embodiments, in the two-component waterborne polyurethane coating, the component A includes the following components, measured by weight: 30-40 parts of hydroxy acrylate, 1-5 parts of acrylic monomer, 34-46 parts of acrylate monomer, 18-30 parts of functional monomer, 2-5 parts of initiator, 1-3 parts of chain transfer agent, 3-8 parts of neutralizer, 60-90 parts of organic solvent and 30-500 parts of water.

[0010] In some of the embodiments, in the two-component waterborne polyurethane coating, the first monomer includes at least one of versatate vinyl carbonate and tert-butyl methacrylate.

[0011] In some of the embodiments, in the two-component waterborne polyurethane coating, the mass ratio of the first monomer to the second monomer is 0.2-0.8:1.

[0012] In some of the embodiments, in the two-component waterborne polyurethane coating, the hydroxyacrylate is at least one of hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate and hydroxypropyl acrylate; and / or

[0013] The acrylic monomer includes at least one of acrylic acid and methacrylic acid; and / or

[0014] The acrylic acid ester monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate and butyl methacrylate.

[0015] In some of the embodiments, in the two-component waterborne polyurethane coating, the initiator includes at least one of di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl hydroperoxide and tert-butyl peroxy-3,5,5-trimethylhexanoate; and / or

[0016] The chain transfer agent comprises at least one of dodecyl mercaptan and 2,4-diphenyl-4-methyl-1-pentene; and / or

[0017] The neutralizing agent comprises at least one of N,N-dimethylethanolamine, triethanolamine and triethylamine; and / or

[0018] The organic solvent includes at least one of xylene, ethylene glycol butyl ether, ethyl acetate, solvent oil, toluene, propylene glycol methyl ether acetate and dipropylene glycol methyl ether acetate.

[0019] In some embodiments, in the two-component waterborne polyurethane coating, the isocyanate curing agent includes a structural fragment represented by formula (I):

[0020] .

[0021] In some embodiments, in the two-component waterborne polyurethane coating, the solid content of component A is 45% to 50%; and / or

[0022] The mass content of hydroxyl group in component A is 3.5% to 4.3%; and / or

[0023] The viscosity of the component A is 500 mPa.s to 2000 mPa.s.

[0024] In some of the embodiments, in the two-component waterborne polyurethane coating, the mass ratio of the component A to the component B is 4-6:1.

[0025] The second aspect of the present application provides a method for preparing a two-component waterborne polyurethane coating, comprising the following steps:

[0026] Providing raw materials according to the components of the above two-component waterborne polyurethane coating;

[0027] Mixing part of the acrylic acid ester monomer, part of the hydroxy acrylic acid, part of the functional monomer, part of the initiator and part of the chain transfer agent to obtain a first mixed solution;

[0028] Mixing acrylic monomers, remaining acrylic ester monomers, remaining hydroxy acrylic acid, acrylic monomers, remaining functional monomers, part of the initiator and remaining chain transfer agent to obtain a second mixed solution;

[0029] The organic solvent is heated to 120° C. to 150° C., and the first mixed solution is added thereto, and then the second mixed solution is added thereto for polymerization reaction to obtain a reaction solution;

[0030] After mixing the reaction solution with a neutralizing agent, water is added to obtain component A;

[0031] Weigh the isocyanate curing agent to obtain component B.

[0032] The third aspect of the present application provides a coating product, comprising a coating formed by curing the above-mentioned two-component waterborne polyurethane coating.

[0033] Compared with the prior art, the two-component waterborne polyurethane coating of the present application has the following beneficial effects:

[0034] The two-component waterborne polyurethane coating of the present application comprises a first monomer and a second monomer of a specific type as functional monomers in a component A, based on hydroxy acrylate, acrylic monomer and acrylic ester monomer, wherein the first monomer comprises an ester having a tertiary carbon structure with a main carbon chain of 4 to 6 carbon atoms, and the second monomer comprises di-tertiary carbon isocyanuric acid glyceryl ester, which has a large molecular volume, is conducive to the compatibility and shielding effect of the component A and the isocyanate curing agent of the component B, so that the isocyanate curing agent of the component B reacts preferentially with the component A, thereby inhibiting the reaction of the isocyanate curing agent with water, and finally effectively improving the selectivity of the reaction between the isocyanate curing agent and the component A, effectively reducing the formation of urea bonds, and having a high crosslinking density, thereby effectively improving the weather resistance of the two-component waterborne polyurethane coating. At the same time, the second monomer di-tertiary carbon isocyanuric acid glyceryl ester has a long-chain structure, which can greatly reduce the amount of solvent used, and is conducive to the water resistance, salt spray resistance and aging resistance of the two-component waterborne polyurethane coating. DETAILED DESCRIPTION

[0035] The present application will be further described in detail below in conjunction with the embodiments and examples. It should be understood that these embodiments and examples are only used to illustrate the present application and are not used to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present application more thorough and comprehensive. It should also be understood that the present application can be implemented in many different forms, and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present application, and the equivalent form obtained also falls within the protection scope of the present application. For example, the features described or described as part of an embodiment can be combined in another embodiment in a suitable manner to produce a new embodiment. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present application, and it should be understood that the present application can be implemented without one or more of these details.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing implementation modes and embodiments and are not intended to limit this application.

[0037] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0038] In the present application, "plurality", "multiple", "multiple times", etc., unless otherwise specified, refer to a quantity greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.

[0039] As used herein, "combination thereof", "any combination thereof", "any combination thereof" etc. include all suitable combinations of any two or more of the listed items.

[0040] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.

[0041] Herein, "preferred", "better", "more preferred", and "suitable" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of this application. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.

[0042] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0043] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0044] In the present application, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0045] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0046] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.

[0047] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0048] In this application, the term "room temperature" or "normal temperature" generally refers to 4°C to 35°C, for example, 20°C ± 5°C. In some embodiments of this application, "room temperature" or "normal temperature" refers to 10°C to 30°C. In some embodiments of this application, "room temperature" or "normal temperature" refers to 20°C to 30°C.

[0049] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 3~5 h means that the units of the left endpoint "3" and the right endpoint "5" are both h (hours).

[0050] All documents mentioned in this application are cited as references in this application, just as each document is cited as reference separately. Unless they conflict with the invention purpose and / or technical solution of this application, the cited documents involved in this application are cited with all contents and all purposes. When the cited documents are involved in this application, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the cited documents are involved in this application, the examples and preferred methods of the cited relevant technical features can also be incorporated into this application as references, but are limited to the implementation of this application. It should be understood that when the cited content conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.

[0051] The mass or weight of the relevant components mentioned in the specification of the embodiments of the present application may not only refer to the specific content of each component, but also indicate the proportional relationship of the mass or weight between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the specification of the embodiments of the present application, it is within the scope disclosed in the specification of the embodiments of the present application. Specifically, the mass or weight described in the specification of the embodiments of the present application may be units known in the chemical industry such as μg, mg, g, and kg.

[0052] According to analysis, the main reasons why the weather resistance of traditional two-component water-based acrylic polyurethane coatings is poorer than that of two-component solvent-based acrylic polyurethane coatings are:

[0053] Under the same hydroxyl value, the crosslinking density of traditional two-component water-based acrylic polyurethane coatings is usually lower than that of two-component solvent-based acrylic polyurethane coatings. This is because in two-component water-based acrylic polyurethane coatings, part of the water-based polyurethane curing agent is consumed by water. Even if the water-based polyurethane curing agent is excessive, the crosslinking density is still lower than that of oily acrylic resin, which ultimately affects weather resistance. At the same time, the water-based polyurethane curing agent reacts with water to form urea bonds, which also affects weather resistance.

[0054] One embodiment of the present application provides a two-component waterborne polyurethane coating, including component A and component B;

[0055] Component A includes the following components by mass: 20-40 parts of hydroxy acrylate, 1-8 parts of acrylic monomer, 30-50 parts of acrylate monomer, 10-40 parts of functional monomer, 0.05-5 parts of initiator, 0.05-5 parts of chain transfer agent, 1-10 parts of neutralizer, 30-100 parts of organic solvent and 30-500 parts of water; the functional monomer includes a first monomer and a second monomer, the first monomer includes an ester containing a tertiary carbon structure with a main carbon chain of 4-6 carbon atoms, and the second monomer includes di-tertiary carbon isocyanuric acid glyceryl ester;

[0056] Component B includes an isocyanate curing agent.

[0057] The two-component waterborne polyurethane coating of the present application comprises a first monomer and a second monomer of a specific type as functional monomers in a component A, based on hydroxy acrylate, acrylic monomer and acrylic ester monomer, wherein the first monomer comprises an ester having a tertiary carbon structure with a main carbon chain of 4 to 6 carbon atoms, and the second monomer comprises di-tertiary carbon isocyanuric acid glyceryl ester, which has a large molecular volume, is conducive to the compatibility and shielding effect of the component A and the isocyanate curing agent of the component B, so that the isocyanate curing agent of the component B reacts preferentially with the component A, thereby inhibiting the reaction of the isocyanate curing agent with water, and finally effectively improving the selectivity of the reaction between the isocyanate curing agent and the component A, effectively reducing the formation of urea bonds, and having a high crosslinking density, thereby effectively improving the weather resistance of the two-component waterborne polyurethane coating. At the same time, the second monomer di-tertiary carbon isocyanuric acid glyceryl ester has a long-chain structure, which can greatly reduce the amount of solvent used, and is conducive to the water resistance, salt spray resistance and aging resistance of the two-component waterborne polyurethane coating.

[0058] It can be understood that in component A of the two-component waterborne polyurethane coating, the mass fraction of hydroxy acrylate includes but is not limited to 20 parts, 22 parts, 25 parts, 28 parts, 30 parts, 32 parts, 35 parts, 38 parts, and 40 parts; the mass fraction of acrylic monomer includes but is not limited to 1 part, 2 parts, 3 parts, 5 parts, 6 parts, and 8 parts; the mass fraction of acrylate monomer includes but is not limited to 30 parts, 32 parts, 34 parts, 35 parts, 36 parts, 38 parts, 40 parts, 42 parts, 45 parts, 46 parts, 48 ​​parts, and 50 parts; the mass fraction of functional monomer includes but is not limited to 10 parts, 15 parts, 18 parts, 20 parts, 25 parts, 30 parts, 35 parts, and 40 parts; the mass fraction of initiator includes but is not limited to 0.05 parts, 0.1 The mass fractions of chain transfer agent include but are not limited to 0.05 parts, 0.1 parts, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts; the mass fractions of neutralizer include but are not limited to 1 parts, 2 parts, 3 parts, 5 parts, 8 parts, 10 parts; the mass fractions of organic solvent include but are not limited to 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts, 100 parts; the mass fractions of water include but are not limited to 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, 200 parts, 300 parts, 400 parts, 500 parts; in some examples, it can be within the range consisting of any two of these point values ​​as end values, the same below.

[0059] A tertiary carbon structure refers to a carbon atom that has no hydrogen atom directly attached to it.

[0060] In some of the examples, in a two-component waterborne polyurethane coating, component A includes the following components, calculated by weight: 30-40 parts of hydroxy acrylate, 1-5 parts of acrylic monomer, 34-46 parts of acrylate monomer, 18-30 parts of functional monomer, 2-5 parts of initiator, 1-3 parts of chain transfer agent, 3-8 parts of neutralizer, 60-90 parts of organic solvent and 30-500 parts of water.

[0061] In some of the examples, in the two-component waterborne polyurethane coating, the first monomer includes at least one of acrylonitrile and acrylamide.

[0062] In some of the examples, in the two-component waterborne polyurethane coating, the mass ratio of the first monomer to the second monomer is 0.2~0.8:1.

[0063] It can be understood that the mass ratio of the first monomer to the second monomer includes but is not limited to 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, and 0.8:1.

[0064] In some of the examples, in the two-component waterborne polyurethane coating, the mass ratio of the first monomer to the second monomer is 0.5-0.8:1.

[0065] In some of the examples, in the two-component waterborne polyurethane coating, the mass ratio of the first monomer to the second monomer is 0.5~0.6:1.

[0066] In some of the examples, the two-component waterborne polyurethane coating includes at least one of hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate and hydroxypropyl acrylate.

[0067] In some of the examples, in the two-component waterborne polyurethane coating, the acrylic monomer includes at least one of acrylic acid and methacrylic acid.

[0068] In some of the examples, in the two-component waterborne polyurethane coating, the acrylate monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate and butyl methacrylate.

[0069] In some of the examples, in the two-component waterborne polyurethane coating, the initiator includes at least one of di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl hydroperoxide, and tert-butyl peroxy-3,5,5-trimethylhexanoate.

[0070] In order to pursue a higher solid content, the amount of initiator used in waterborne polyurethane coatings is much greater than that in solvent-based polyurethane coatings, and excessive use of initiators will reduce weather resistance; using specific types of initiators can reduce the amount of initiator used, thereby effectively avoiding the impact on weather resistance caused by using more initiators.

[0071] The above initiator does not contain a benzene ring, and does not contain a benzene ring or other chromophores after decomposition.

[0072] In some of the examples, in the two-component waterborne polyurethane coating, the chain transfer agent includes at least one of dodecyl mercaptan and 2,4-diphenyl-4-methyl-1-pentene.

[0073] In some of the examples, in the two-component waterborne polyurethane coating, the neutralizer includes at least one of N,N-dimethylethanolamine, triethanolamine and triethylamine.

[0074] In some of the examples, in the two-component waterborne polyurethane coating, the organic solvent includes at least one of xylene, ethylene glycol butyl ether, ethyl acetate, solvent oil, toluene, propylene glycol methyl ether acetate and dipropylene glycol methyl ether acetate.

[0075] In some of these examples, in a two-component waterborne polyurethane coating, the isocyanate curing agent includes a structural fragment represented by formula (I):

[0076] .

[0077] The isocyanate curing agent containing a specific main structure is similar to the structure of di-tert-isocyanuric acid glycerol ester, which effectively improves the selectivity of the reaction between the isocyanate curing agent and component A, effectively reduces the formation of urea bonds, and has a high cross-linking density, thereby effectively improving the weather resistance of the two-component waterborne polyurethane coating.

[0078] In some of these examples, the solids content of component A in a two-component waterborne polyurethane coating is 45% to 50%.

[0079] It will be appreciated that the amount of water used in component A can be determined based on the solid content of component A.

[0080] In some of these examples, in two-component waterborne polyurethane coatings, the hydroxyl mass content of component A is 3.5%~4.3%.

[0081] In some of these examples, in two-component waterborne polyurethane coatings, the viscosity of component A is 500 mPa.s~2000 mPa.s.

[0082] In some of these examples, in two-component waterborne polyurethane coatings, the mass ratio of component A to component B is 4 to 6:1.

[0083] It can be understood that the mass ratio of component A to component B includes but is not limited to 4:1, 5:1, and 6:1.

[0084] The two-component waterborne polyurethane coating provided in the present application has high hydroxyl content, high solid content, low viscosity, high gloss, outstanding aging resistance, and QUV ≥ 2000 hours.

[0085] An embodiment of the present application provides a method for preparing a two-component waterborne polyurethane coating, comprising the following steps:

[0086] Providing raw materials according to the components of the above two-component waterborne polyurethane coating;

[0087] Mixing part of the acrylic acid ester monomer, part of the hydroxy acrylic acid, part of the functional monomer, part of the initiator and part of the chain transfer agent to obtain a first mixed solution;

[0088] Mixing acrylic monomers, remaining acrylic ester monomers, remaining hydroxy acrylic acid, acrylic monomers, remaining functional monomers, part of the initiator and remaining chain transfer agent to obtain a second mixed solution;

[0089] The organic solvent is heated to 120° C. to 150° C., and after adding the first mixed solution, the second mixed solution is added to carry out polymerization reaction to obtain a reaction solution;

[0090] After mixing the reaction solution with the neutralizing agent, water is added to obtain component A;

[0091] Weigh the isocyanate curing agent to obtain component B.

[0092] The two-component waterborne polyurethane coating prepared by the preparation method of the two-component waterborne polyurethane coating of the present application has good weather resistance, water resistance, salt spray resistance and aging resistance.

[0093] In the presence of an initiator, free radical polymerization occurs between the monomers.

[0094] One embodiment of the present application provides a coated product, including a coating formed by curing the above-mentioned two-component waterborne polyurethane coating.

[0095] The coated product provided in the present application includes a coating formed after curing of the above-mentioned two-component water-based polyurethane coating, which can give the coated product good weather resistance, water resistance, salt spray resistance and aging resistance, effectively extending the service life of the coated product.

[0096] It can be understood that coated products include but are not limited to rail transit vehicles, automobiles, high-end engineering machinery, flooring, wooden products, etc.

[0097] The present application is further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present application are not limited thereto.

[0098] In the following embodiments, the Chinese names corresponding to the English abbreviations are:

[0099] MMA: methyl methacrylate;

[0100] BA: butyl acrylate;

[0101] MBA: butyl methacrylate;

[0102] TBA: tert-butyl (meth)acrylate;

[0103] HEMA: hydroxyethyl methacrylate;

[0104] HPMA: Hydroxypropyl methacrylate;

[0105] MAA: methacrylic acid;

[0106] VV-10: tert-butyl vinyl carbonate;

[0107] Ditertiary carbon isocyanurate glycerol ester: from Jinjia New Materials, model EWA-2;

[0108] Example 1

[0109] Component A, calculated by mass, includes: hydroxy acrylate (24 parts of HEMA, 9 parts of HPMA), acrylic monomer (3 parts of MAA), acrylate monomer (24 parts of MMA, 19 parts of BA, 3 parts of MBA), first monomer (8 parts of TBA), second monomer (10 parts of EWA-2), initiator di-tert-butyl peroxide 3 parts, chain transfer agent dodecyl mercaptan 1 part, neutralizer dimethylethanolamine 5 parts, organic solvent xylene 80 parts and balance water to a solid content of 45%; wherein, the mass ratio of the first monomer to the second monomer is 0.8:1.

[0110] Component B: Isocyanate curing agent (Covestro waterborne polyurethane curing agent XP2655).

[0111] The preparation method of component A is as follows:

[0112] (1) BA, 70 wt% HEMA, 70 wt% HPMA, 50 wt% EWA-2, 50 wt% TBA, part of the initiator and the chain transfer agent were mixed uniformly to prepare a first mixed solution;

[0113] (2) MMA, MBA, 30 wt% HEMA, 30 wt% HPMA, MAA, 50 wt% EWA-2, 50 wt% TBA), part of the initiator and the chain transfer agent are mixed uniformly to prepare a second mixed solution;

[0114] (3) Heat xylene to 135°C, add the first mixed solution dropwise for 2 h, and keep warm for 1 h;

[0115] (4) Continue to mix the second solution for 2 h, keep warm for 2 h; add the remaining initiator and keep warm for another 2 h; cool to 40 °C, add the neutralizer; then add water to obtain component A.

[0116] Example 2

[0117] The method is basically the same as Example 1, except that component A, by weight, includes: hydroxy acrylate (24 parts of HEMA, 9 parts of HPMA), acrylic monomer (3 parts of MAA), acrylate monomer (17 parts of MMA, 14 parts of BA, 3 parts of MBA), a first monomer (10 parts of TBA), a second monomer (20 parts of EWA-2), an initiator of di-tert-butyl peroxide 3 parts, a chain transfer agent of dodecyl mercaptan 1 part, a neutralizing agent of dimethylethanolamine 5 parts, an organic solvent of xylene 80 parts, and the balance of water to a solid content of 45%; wherein the mass ratio of the first monomer to the second monomer is 0.5:1.

[0118] Example 3

[0119] It is basically the same as Example 1, except that in component A, the total mass of the first monomer and the second monomer is the same as that in Example 1, only the first monomer (3 parts of TBA) and the second monomer (15 parts of EWA-2) are present, and the mass ratio of the first monomer to the second monomer is 0.2:1.

[0120] Component A, calculated by mass, includes: hydroxy acrylate (24 parts of HEMA, 9 parts of HPMA), acrylic monomer (3 parts of MAA), acrylate monomer (24 parts of MMA, 19 parts of BA, 3 parts of MBA), first monomer (3 parts of TBA), second monomer (15 parts of EWA-2), initiator di-tert-butyl peroxide 3 parts, chain transfer agent dodecyl mercaptan 1 part, neutralizer dimethylethanolamine 5 parts, organic solvent xylene 80 parts and balance water to a solid content of 45%; wherein, the mass ratio of the first monomer to the second monomer is 0.8:1.

[0121] Comparative Example 1

[0122] The method is basically the same as Example 1, except that in component A, the second monomer EWA-2 is replaced with an equal mass of caprolactone methacrylate.

[0123] Control group

[0124] Two-component solvent-based acrylic polyurethane coating: Component A is resin provided by Bayer A870, and component B is Covestro XP3900.

[0125] The components A and B of the embodiments and comparative examples were mixed in a mass ratio of 5:1, and the mixed two-component waterborne polyurethane coating was coated to form a dry film with a thickness of 30 μm, and tested (according to HG / T 4761-2014). The results are shown in Table 1.

[0126] Table 1

[0127]

[0128] It can be seen from Table 1 that the two-component waterborne polyurethane coatings prepared in each embodiment have good weather resistance and can achieve the weather resistance of the two-component solvent-based acrylic polyurethane coating; while in Comparative Example 1, the second monomer EWA-2 is replaced with an equal mass of caprolactone methacrylate, and the weather resistance is significantly reduced, and the gloss is reduced.

[0129] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0130] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A two-component waterborne polyurethane coating, It is characterized in that It includes component A and component B; The component A comprises the following components by mass: 20-40 parts of hydroxy acrylate, 1-8 parts of acrylic monomer, 30-50 parts of acrylate monomer, 10-40 parts of functional monomer, 0.05-5 parts of initiator, 0.05-5 parts of chain transfer agent, 1-10 parts of neutralizer, 30-100 parts of organic solvent and 30-500 parts of water; the functional monomer comprises a first monomer and a second monomer, the first monomer comprises an ester containing a tertiary carbon structure with a main carbon chain of 4-6 carbon atoms, and the second monomer comprises di-tertiary carbon isocyanuric acid glyceryl ester; The B component includes an isocyanate curing agent.

2. The two-component waterborne polyurethane coating according to claim 1, It is characterized in that Calculated by mass, the component A includes the following components: 30-40 parts of hydroxy acrylate, 1-5 parts of acrylic monomer, 34-46 parts of acrylate monomer, 18-30 parts of functional monomer, 2-5 parts of initiator, 1-3 parts of chain transfer agent, 3-8 parts of neutralizer, 60-90 parts of organic solvent and 30-500 parts of water.

3. The two-component waterborne polyurethane coating according to claim 1, It is characterized in that The first monomer includes at least one of versatate vinyl carbonate and tert-butyl methacrylate.

4. The two-component waterborne polyurethane coating according to claim 1, It is characterized in that The mass ratio of the first monomer to the second monomer is 0.2-0.8:

1.

5. The two-component waterborne polyurethane coating according to any one of claims 1 to 4, It is characterized in that At least one of the hydroxyacrylate-based hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate and hydroxypropyl acrylate; and / or The acrylic monomer includes at least one of acrylic acid and methacrylic acid; and / or The acrylic acid ester monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate and butyl methacrylate.

6. The two-component waterborne polyurethane coating according to any one of claims 1 to 4, It is characterized in that The initiator comprises at least one of di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl hydroperoxide and tert-butyl peroxy-3,5,5-trimethylhexanoate; and / or The chain transfer agent comprises at least one of dodecyl mercaptan and 2,4-diphenyl-4-methyl-1-pentene; and / or The neutralizing agent comprises at least one of N,N-dimethylethanolamine, triethanolamine and triethylamine; and / or The organic solvent includes at least one of xylene, ethylene glycol butyl ether, ethyl acetate, solvent oil, toluene, propylene glycol methyl ether acetate and dipropylene glycol methyl ether acetate.

7. The two-component waterborne polyurethane coating according to any one of claims 1 to 4, It is characterized in that The isocyanate curing agent includes a structural fragment shown in formula (I): 。 8. The two-component waterborne polyurethane coating according to any one of claims 1 to 4, It is characterized in that The solid content of component A is 45% to 50%; and / or The mass content of hydroxyl group in component A is 3.5% to 4.3%; and / or The viscosity of component A is 500 mPa.s to 2000 mPa.s; and / or The mass ratio of the component A to the component B is 4-6:

1.

9. A method for preparing a two-component waterborne polyurethane coating, It is characterized in that The following steps are involved: Providing raw materials for the components of the two-component waterborne polyurethane coating according to any one of claims 1 to 8; Mixing part of the acrylic acid ester monomer, part of the hydroxy acrylic acid, part of the functional monomer, part of the initiator and part of the chain transfer agent to obtain a first mixed solution; Mixing acrylic monomers, remaining acrylic ester monomers, remaining hydroxy acrylic acid, acrylic monomers, remaining functional monomers, part of the initiator and remaining chain transfer agent to obtain a second mixed solution; The organic solvent is heated to 120° C. to 150° C., and the first mixed solution is added thereto, and then the second mixed solution is added thereto for polymerization reaction to obtain a reaction solution; After mixing the reaction solution with a neutralizing agent, water is added to obtain component A; Weigh the isocyanate curing agent to obtain component B.

10. A coated product, It is characterized in that The invention comprises a coating formed by curing the two-component waterborne polyurethane coating as claimed in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Water-based two-component polyurethane paint

    CN103540253A

  • Manufacturing and using method of high-hardness stain-resistant automobile water-based two-component polyurethane coating with core-shell structure

    CN113122119A

  • Hydroxyl polyacrylate dispersion, preparation method thereof, high-performance water-based two-component polyurethane coating and preparation method of high-performance water-based two-component polyurethane coating

    CN114349896A

  • Water-based hydroxyl acrylic acid dispersion and preparation method and application thereof

    CN117777364A