High-weather-resistance flexible fabric membrane material and preparation method thereof

Through the seven-layer film structure and the hydrogen bonding and cross-linking structure of modified polyvinyl chloride and polyvinylidene fluoride, the heat resistance and adhesion of flexible fabric films in harsh environments are solved, and high weather resistance and Good UV infrared barrier performance.

CN119081560AInactive Publication Date: 2024-12-06SHENZHEN ZHONGDE MEMBRANE STRUCTURE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411539546.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing flexible fabric films have poor heat resistance under severe weather conditions, especially PVC materials are prone to decomposition at high temperatures, and the adhesion between polyvinyl chloride and polyvinylidene fluoride is poor and it is difficult to form an effective coating, which affects its ultraviolet Infrared barrier performance.

Method used

Using a seven-layer film structure, including polyvinylidene fluoride coating layer, modified polyvinyl chloride layer, adhesive layer, base cloth layer, adhesive layer, polyvinyl chloride layer and acrylic treatment layer, modified polyvinyl chloride and Hydrogen bond formation and unsaturated double bond crosslinking structure of polyvinylidene fluoride enhance bonding and weather resistance, and use nanotitanium dioxide and alumina ceramic powder as inorganic fillers to improve the wear resistance, toughness and tensile properties of the film .

Benefits of technology

It realizes a flexible fabric film with high weather resistance and good UV infrared barrier properties, enhances the adhesion between the polyvinyl chloride layer and the polyvinylidene fluoride coating layer, and improves the tensile strength and heat resistance of the film material. At the same time, the problem of poor mutual solubility of heat stabilizers is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081560A_ABST
    Figure CN119081560A_ABST
Patent Text Reader

Abstract

The invention relates to the field of new energy, in particular to a high-weather-resistance flexible fabric membrane material and a preparation method thereof.The flexible fabric membrane material comprises seven membrane layers which sequentially comprise a polyvinylidene fluoride membrane layer, a polyvinyl chloride layer, a bonding layer, a base cloth layer, a bonding layer, a polyvinyl chloride layer and an acrylic treatment layer from top to bottom; the polyvinyl chloride layer comprises the following raw materials in parts by mass: 80-90 parts of modified polyvinyl chloride, 45-47 parts of a plasticizer, 2-4 parts of a lubricant and 10-12 parts of nano titanium dioxide. The flexible fabric membrane material disclosed by the invention has the advantages of good adhesion, weather resistance, good ultraviolet and infrared barrier property, better wear resistance, toughness and tensile property, and wider shape application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy, and in particular to a highly weather-resistant flexible fabric membrane material and a preparation method thereof. Background Art

[0002] With the continuous development and innovation of my country's materials industry, the types of materials are gradually increasing. Among them, flexible fabric membrane materials have received widespread attention and application in many fields such as environmental protection closure of industrial storage silos, closure of sewage pools, contaminated soil, and ore. It is supported by air and forms a stable spatial structure by filling the membrane with gas. Flexible fabric membrane materials are supported by air and their own weight is much lower than traditional membrane materials. They are relatively easy to install and disassemble, which makes them very suitable for temporary or mobile large-scale equipment, environmental protection equipment, etc. Therefore, they can significantly reduce the burden on the foundation and reduce costs. Although flexible fabric membrane materials have many advantages, their disadvantages are also obvious. For example, membrane materials have a certain strength, but they may not be as good as traditional large equipment. The materials used are durable, especially under adverse weather conditions. The main PVC material will decompose in some high temperature weather due to its poor heat resistance, which seriously affects the use of the air film. In response to the problem of poor heat resistance of PVC, the patent with publication number CN110885520B discloses "a high hardness, oil-resistant and heat-resistant PVC material" which solves the problem of poor heat resistance of PVC by adding fillers such as heat stabilizers. For example, the patent with publication number CN116589807B discloses "a heat-resistant PVC film and its preparation method and application" which also solves the problem of poor heat resistance of PVC by adding heat-resistant modifiers. However, this method requires strict control of the compatibility of the heat stabilizer and the matrix, otherwise it will seriously affect the use of PVC.

[0003] The patent with publication number CN105754040B discloses "high fluidity heat-resistant PVC resin and preparation method thereof". The applicant synthesized a new type of heat-resistant PVC resin by using polyvinyl chloride resin, bridge compound, functional monomer and initiator as main raw materials. For example, the patent with publication number CN109438876A discloses "a heat-resistant and environmentally friendly PVC pharmaceutical packaging material". The thermal stability of the PVC material is improved by functionalizing the PVC resin with maleic anhydride. Studies have shown that the modification methods of the above two patents can effectively solve the problem of poor miscibility between PVC and heat stabilizers.

[0004] However, in the application of flexible fabric membranes, higher requirements are put forward for the heat resistance of PVC. Therefore, researchers are not limited to the heat resistance modification of PVC. They further enhance the resistance of PVC to ultraviolet and infrared aging by coating PVC. For example, CN210792355U discloses "a kind of corrosion-resistant sewage pool membrane material" with polyester woven fabric as the base fabric, and a colored PVC plastic slurry layer and a white PVC plastic slurry layer are provided on the upper and lower surfaces. A PVDF surface layer is provided on one side of the composite material, and a PVDF film layer is attached on the other side to form a membrane material with good light-shielding performance. For example, CN202192822U discloses "polyvinyl chloride biogas agricultural membrane" with a polyvinyl chloride adhesive layer and a polyvinyl chloride film layer coated on the upper and lower sides of the middle skeleton layer, and an acrylic film layer is coated on the reverse side, and a polyvinylidene fluoride film layer is coated on the front side. The membrane material prepared by this method has the effects of high ultraviolet resistance and good corrosion resistance. However, studies have shown that the poor adhesion between polyvinyl chloride and polyvinylidene fluoride makes it difficult to effectively coat polyvinylidene fluoride on polyvinyl chloride. The above patents fail to mention and solve this problem.

[0005] Therefore, it is urgent to develop a flexible fabric membrane material with good lamination adhesion, weather resistance, and good ultraviolet and infrared barrier properties. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a highly weather-resistant flexible fabric membrane and a preparation method thereof. The flexible fabric membrane of the present invention has good film adhesion, weather resistance, ultraviolet and infrared barrier properties, and also has good wear resistance, toughness and tensile properties, and has a wider range of shapes and applications.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: On one hand, the present invention provides a highly weather-resistant flexible fabric membrane material, the flexible fabric membrane material comprises seven membrane layers, which include, from top to bottom, a polyvinylidene fluoride coating layer, a polyvinyl chloride layer, an adhesive layer, a base fabric layer, an adhesive layer, a polyvinyl chloride layer and an acrylic treatment layer; The polyvinyl chloride layer comprises the following raw materials in parts by weight: 80-90 parts of modified polyvinyl chloride, 45-47 parts of plasticizer, 2-4 parts of lubricant and 10-12 parts of nano titanium dioxide.

[0008] The invention enhances the weather resistance and ultraviolet and infrared barrier properties of the flexible fabric membrane material through the synergy of multiple membrane layers, and improves its wear resistance, toughness and tensile properties at the same time.

[0009] In some embodiments, the inorganic filler is a mixture of nano titanium dioxide and aluminum hydroxide.

[0010] Preferably, the inorganic filler is a mixture of alumina ceramic powder and nano-silicon dioxide, and the mass ratio of the two is 1:(0.2~0.5).

[0011] Preferably, the inorganic filler is a mixture of alumina ceramic powder and nano-silicon dioxide, and the mass ratio of the two is 1:0.3.

[0012] In some embodiments, the plasticizer is one or more of diisooctyl adipate, triphenyl phosphate, and diisononyl phthalate.

[0013] In some embodiments, the lubricant is polyethylene wax.

[0014] In some embodiments, the base fabric layer is polyethylene terephthalate.

[0015] In some embodiments, the acrylic treatment layer includes the following raw materials in parts by weight: 88-90 parts of polymethyl methacrylate, 8-10 parts of diisononyl phthalate, 0.2-0.3 parts of polyethylene wax, and 1-2 parts of nano titanium dioxide.

[0016] In some embodiments, the polyvinylidene fluoride coating layer includes the following raw materials in parts by weight: 80-90 parts of modified polyvinylidene fluoride, 20-24 parts of titanium dioxide grafted modified aramid fiber, 10-14 parts of polymethyl methacrylate, 1-5 parts of inorganic filler, 30-40 parts of deionized water and 30-40 parts of anhydrous ethanol.

[0017] Preferably, the polyvinylidene fluoride coating layer comprises the following raw materials in parts by weight: 85 parts of modified polyvinylidene fluoride, 22 parts of titanium dioxide grafted modified aramid fiber, 12 parts of polymethyl methacrylate, 3 parts of inorganic filler and 35 parts of deionized water.

[0018] In some embodiments, the method for preparing the modified polyvinylidene fluoride comprises the following steps: A1. Mix fumaric acid, 1,3-dihydroxyacetone and the first solvent, add dilute sulfuric acid, heat to 60-70°C and stir for 12-16 hours, cool to 0-5°C after the reaction, add saturated sodium bicarbonate solution until no bubbles are generated, concentrate under reduced pressure, extract with ethyl acetate, concentrate the organic phase under reduced pressure and dry, and obtain the compound shown in Formula I (I); A2, the compound represented by formula I in step A1, 2-aminoethylphosphonic acid, piperidine, trimethyl orthoformate, and the first solvent are mixed, the temperature is raised to 60-70°C and stirred at a constant temperature for 6-8 hours, after the reaction is completed, the mixture is concentrated and dried under reduced pressure, and column chromatography is performed to obtain the compound represented by formula II (II); A3. Mix the compound represented by formula II in step A2, monomeric vinylidene fluoride, sodium dodecyl sulfate and water, then add potassium persulfate and sodium sulfite and stir for 10-15 minutes, raise the temperature to 60-70°C and stir at a constant temperature for 6.5-7.5 hours, centrifuge and filter after the reaction, wash with anhydrous ethanol to obtain modified polyvinylidene fluoride.

[0019] Preferably, in step A1, the volume of the first solvent is 7 times the total mass of fumaric acid and 1,3-dihydroxyacetone.

[0020] Preferably, in step A2, the volume of the first solvent is 8 times the mass of the compound represented by formula I.

[0021] Preferably, in step A3, the volume of the deionized water is 25 times the mass of the compound represented by formula II.

[0022] In some embodiments, the method for preparing the titanium dioxide grafted modified aramid fiber comprises the following steps: B1, soaking the aramid fiber in an ethanol solution for ultrasonic treatment, and then washing and drying with deionized water to obtain pretreated aramid fiber; B2, passing the pretreated aramid fiber in step B1 through a low-temperature plasma generator, controlling the argon gas flow rate to 8-9 mL / min, and treating for 4-6 min at a plasma discharge power of 75-85 W to obtain a surface-treated aramid fiber; B3, mixing butyl titanate, glacial acetic acid and anhydrous ethanol, stirring at room temperature for 30-40 minutes to obtain a mixed solution A; B4, mixing the second anhydrous ethanol and deionized water and adjusting the pH to 3-4 with dilute hydrochloric acid to obtain a mixed solution B; B5, at room temperature, adding the mixed solution B in step B4 to the mixed solution A in step B3 at a rate of 4-6 mL / min, and stirring at room temperature for 2-3 h to obtain a titanium dioxide gel; B6. Immerse the surface treated aramid fiber in step B2 in the mixture of titanium dioxide gel and propylene oxide in step B5, place it in an oven at 100-140° C. for heat treatment for 30-40 min, remove the surface treated aramid fiber in step B2, and dry it to obtain titanium dioxide grafted modified aramid fiber.

[0023] Preferably, the method for preparing the titanium dioxide grafted modified aramid fiber comprises the following steps, calculated by weight: B1, soaking 20 parts of aramid fibers in a 95% volume concentration ethanol solution for ultrasonic treatment, and then washing and drying with deionized water to obtain pretreated aramid fibers; B2, passing the pretreated aramid fiber in step B1 through a low-temperature plasma generator, controlling the argon gas flow rate to 8 mL / min, and treating for 5 min at a plasma discharge power of 80 W to obtain a surface-treated aramid fiber; B3, 100 parts of butyl titanate, 84 parts of glacial acetic acid and 16 parts of anhydrous ethanol were mixed, and stirred at room temperature for 35 minutes to obtain a mixed solution A; B4, 71 parts of anhydrous ethanol and 45 parts of deionized water were mixed and the pH was adjusted to 3 with 10wt% dilute hydrochloric acid to obtain a mixed solution B; B5, at room temperature, the mixed solution B in step B4 was added dropwise to the mixed solution A in step B3 at a rate of 5 mL / min, and stirred at room temperature for 2.5 h to obtain a titanium dioxide gel; B6. Soak the surface treated aramid fiber in step B2 in a mixture of 300 parts of the titanium dioxide gel in step B5 and 12 parts of propylene oxide, place it in an oven at 120° C. for heat treatment for 35 minutes, remove the surface treated aramid fiber in step B2, and dry it to obtain the titanium dioxide grafted modified aramid fiber.

[0024] In some embodiments, the method for preparing the modified polyvinyl chloride comprises the following steps: S1. Mix 2-aminonicotinic acid and triethylamine in tetrahydrofuran, cool to -5~0°C, add p-toluenesulfonyl chloride in tetrahydrofuran dropwise, return to room temperature and continue stirring for 20~24h, concentrate under reduced pressure and pass through column chromatography to obtain compound A; S2, mixing compound A, 1,3-benzenedimethanol and anhydrous methanol in step S1, adding dilute sulfuric acid, heating to 60-70° C. and stirring at constant temperature for 8-12 hours to obtain compound B; S3, 0.45 g of magnesium metal and 15 ml of anhydrous methanol were mixed, 0.74 g of compound B in step S2 was added, and the mixture was stirred at room temperature for 6 to 8 hours. After filtering, the filtrate was concentrated under reduced pressure to obtain compound C; S4, dissolving maleic anhydride in dichloromethane, adding dilute sulfuric acid thereto and heating to 35-40°C, adding the dichloromethane dilution of compound C in step S3 dropwise thereto, and continuing to stir at a constant temperature for 8-12 hours after the addition is complete. After the reaction is completed, cool to room temperature, concentrate and dry under reduced pressure, and perform column chromatography to obtain a functional monomer; S5, adding the functional monomer in step S4 into deionized water, adding a dispersant and an initiator, heating to 45-50° C., introducing an inert protective gas to replace the air in the reactor, and then introducing vinyl chloride gas, stirring at a constant temperature for 4-6 hours, filtering after the reaction is completed, and obtaining a modified polyvinyl chloride precursor; S6. Add the modified polyvinyl chloride precursor in step S5 into anhydrous ethanol, add a diluted anhydrous ethanol solution of lanthanum nitrate dropwise thereto, then adjust the system pH to 6-7 with aqueous ammonia, stir at room temperature for 4-5 hours, let stand, centrifuge and filter, wash and dry to obtain modified polyvinyl chloride.

[0025] The modified polyvinyl chloride of the present application has good heat resistance and stability, and is mainly obtained through copolymerization modification, avoiding the problem of poor mutual solubility caused by the conventional addition of heat stabilizers. In addition, the applicant unexpectedly discovered that the adhesion between the polyvinyl chloride layer and the polyvinylidene fluoride coating layer of the present application is enhanced, and the tensile strength of the flexible fabric membrane is increased. The reason may be that, on the one hand, the modified polyvinyl chloride structure contains a large number of amide groups, which form stable hydrogen bonds with the polyvinylidene fluoride coating layer, thereby enhancing the adhesion performance of the coating; on the other hand, the functional monomer structure of the present application has an unsaturated double bond structure, which can form a cross-linked structure with vinyl chloride, which not only increases the stability of the modified polyvinyl chloride molecular structure and thereby enhances the heat resistance and stability of the flexible fabric membrane, but also improves the tensile strength of the flexible fabric membrane.

[0026] In some embodiments, in step S2, the molar ratio of compound A to 1,3-benzenedimethanol is 1:(0.4~0.5).

[0027] Preferably, in step S2, the molar ratio of compound A to 1,3-benzenedimethanol is 1:0.45.

[0028] In some embodiments, the molar ratio of the metallic magnesium to the compound B is (2-2.2):1.

[0029] In some embodiments, in step S4, the molar ratio of compound C to maleic anhydride is 1:(2-2.2).

[0030] Preferably, in step S4, the molar ratio of compound C to maleic anhydride is 1:2.1.

[0031] In some embodiments, in step S5, the molar ratio of the functional monomer to the vinyl chloride gas is (0.1-0.3):1.

[0032] Preferably, in step S5, the molar ratio of the functional monomer to the vinyl chloride gas is 0.2:1.

[0033] The applicant can prevent the cross-linking density of the modified polyvinyl chloride from being too high, thereby reducing the flexibility of the flexible fabric membrane material, by adjusting the molar ratio of the functional monomer to the vinyl chloride gas.

[0034] In some embodiments, the adhesive layer is acrylate.

[0035] In some embodiments, the acrylic processing layer includes the following raw materials in parts by weight: 88 to 90 parts of polymethyl methacrylate, 8 to 10 parts of diisononyl phthalate, 1 to 2 parts of titanium dioxide, and 1 to 1.5 parts of a heat stabilizer.

[0036] On the other hand, the present application provides a method for preparing a highly weather-resistant flexible fabric membrane material, comprising the following steps: An adhesive layer is coated on the upper and lower surfaces of the base fabric layer respectively, and then a polyvinyl chloride layer is coated on the surface of the adhesive layer, and hot pressing is performed at 140-150°C for 3-5 minutes to form, and then an acrylic treatment layer is coated on the lower polyvinyl chloride layer, and it is placed at 60-70°C for drying for 10-20 minutes to form, and a polyvinylidene fluoride coating layer is coated on the upper polyvinyl chloride layer, and it is placed at 65-75°C for drying for 20-30 minutes to obtain a highly weather-resistant flexible fabric membrane material.

[0037] In some embodiments, the thickness of the polyvinylidene fluoride coating layer is 20-40 μm; the thickness of the polyvinyl chloride layer is 200-250 μm; the thickness of the adhesive layer is 20-30 μm; the thickness of the base fabric layer is 500-600 μm; and the thickness of the acrylic treatment layer is 70-80 μm.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The flexible fabric membrane material of the present invention has a total of seven layers, which are, from top to bottom, a polyvinylidene fluoride coating layer, a polyvinyl chloride layer, an adhesive layer, a base fabric layer, an adhesive layer, a polyvinyl chloride layer and an acrylic treatment layer. The flexible fabric membrane material is obtained by bonding multiple layers of membrane materials. The flexible fabric membrane material has good weather resistance and ultraviolet and infrared barrier properties, and also has good wear resistance, toughness and tensile properties. In addition, the polyvinylidene fluoride coating layer and the polyvinyl chloride layer have good adhesion and are not easy to separate.

[0040] (2) The modified polyvinyl chloride of the present invention solves the problem of poor heat resistance of conventional polyvinyl chloride, enhances the weather resistance of the flexible fabric membrane, and can enhance the adhesion between the polyvinyl chloride layer and the polyvinylidene fluoride coating layer, and improves the tensile strength of the flexible fabric membrane.

[0041] (3) The present invention can prevent the cross-linking density of the modified polyvinyl chloride from being too high, thereby reducing the flexibility of the flexible fabric membrane material, by selecting a specific molar ratio of functional monomers and vinyl chloride gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the structure of highly weather-resistant flexible fabric membrane Figure identification: 1-polyvinylidene fluoride coating layer; 2-polyvinyl chloride layer; 3-adhesive layer; 4-base fabric layer; 5-acrylic treatment layer. DETAILED DESCRIPTION

[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] In the following preparation examples, embodiments and comparative examples, aramid fiber was purchased from Jiangxi Shuobang New Material Technology Co., Ltd.; polymethyl methacrylate was purchased from Dongguan Zhengtao Plastic Co., Ltd.; alumina ceramic powder was purchased from Hebei Yuechao Wear-Resistant Materials Co., Ltd.; polyvinylidene fluoride was purchased from Dongguan Baojia Plastic Co., Ltd.; polyethylene terephthalate was purchased from Shanghai Qianfu Industrial Co., Ltd.; polymethyl methacrylate was purchased from Shanghai Shunshi Plastic Co., Ltd.; polyethylene wax was purchased from Shanghai Zhenlishi Network Technology Co., Ltd.; polyvinyl chloride was purchased from Weifang Luyang Waterproof Materials Co., Ltd.

[0045] In the following embodiments, the polyvinylidene fluoride coating layer 1 comprises the following raw materials by weight: 85 parts of modified polyvinylidene fluoride, 22 parts of titanium dioxide grafted modified aramid fiber, 12 parts of polymethyl methacrylate, 3 parts of inorganic filler, 35 parts of deionized water and 35 parts of anhydrous ethanol, wherein the modified polyvinylidene fluoride is prepared by Preparation Example 1 described later, the titanium dioxide grafted modified aramid fiber is prepared by Preparation Example 2 described later, and the inorganic filler is a mixture of 2.3 parts of alumina ceramic powder and 0.7 parts of nano-silicon dioxide; The adhesive layer 3 is methyl acrylate; The base fabric layer 4 is polyethylene terephthalate; The acrylic treatment layer 5 includes the following raw materials in parts by weight: 89 parts of polymethyl methacrylate, 9 parts of diisononyl phthalate, 0.2 parts of polyethylene wax and 1.5 parts of nano titanium dioxide.

[0046] Preparation Example 1 The preparation method of modified polyvinylidene fluoride comprises the following steps: A1. Mix 1 mol of fumaric acid, 2.1 mol of 1,3-dihydroxyacetone and 2.1 L of anhydrous ethanol, add 50 g of 47% dilute sulfuric acid, heat to 65°C and stir for 14 h. After the reaction, cool to 3°C, add saturated sodium bicarbonate solution until no bubbles are generated, concentrate under reduced pressure, extract with ethyl acetate, concentrate the organic phase under reduced pressure and dry to obtain the compound shown in Formula I. (I); A2, 1 mol of the compound represented by formula I in step A1, 2.1 mol of 2-aminoethylphosphonic acid, 1.1 mol of piperidine, 1.1 mol of trimethyl orthoformate, and 2 L of anhydrous ethanol were mixed, the temperature was raised to 65°C and stirred at constant temperature for 7 hours, after the reaction was completed, the mixture was concentrated and dried under reduced pressure, and the compound represented by formula II was obtained by column chromatography. (II); A3. Mix 0.05 mol of the compound represented by formula II in step A2, 1 mol of vinylidene fluoride monomer, 0.02 mol of sodium dodecyl sulfate and 600 mL of deionized water, add 0.06 g of potassium persulfate and 0.06 g of sodium sulfite, stir for 13 minutes, heat to 65°C and stir at constant temperature for 7 hours. After the reaction is completed, centrifuge and filter, wash with anhydrous ethanol to obtain modified polyvinylidene fluoride.

[0047] Preparation Example 2 The preparation method of titanium dioxide grafted modified aramid fiber comprises the following steps: B1, soaking 20g of aramid fiber in 100mL of 95% volume concentration ethanol solution for ultrasonic treatment, and then washing and drying with deionized water to obtain pretreated aramid fiber; B2, passing the pretreated aramid fiber in step B1 through a low-temperature plasma generator, controlling the argon gas flow rate to 8 mL / min, and treating for 5 min at a plasma discharge power of 80 W to obtain a surface-treated aramid fiber; B3, 100 mL of butyl titanate, 80 mL of glacial acetic acid, and 20 mL of anhydrous ethanol were mixed, and stirred at room temperature for 35 min to obtain a mixed solution A; B4, 90 mL of anhydrous ethanol and 45 mL of deionized water were mixed and the pH was adjusted to 3 with 10 wt % dilute hydrochloric acid to obtain a mixed solution B; B5, at room temperature, the mixed solution B in step B4 was added dropwise to the mixed solution A in step B3 at a rate of 5 mL / min, and stirred at room temperature for 2.5 h to obtain a titanium dioxide gel; B6. Soak the surface treated aramid fiber in step B2 in a mixture of 300 g of the titanium dioxide gel in step B5 and 12 g of propylene oxide, place it in an oven at 120° C. for heat treatment for 35 min, take out the surface treated aramid fiber in step B2, and dry it to obtain the titanium dioxide grafted modified aramid fiber.

[0048] Preparation Example 3 The preparation method of modified polyvinyl chloride comprises the following steps: S1. Mix 1 mol of 2-aminonicotinic acid and 1 mol of triethylamine in 1.5 L of tetrahydrofuran, cool to -3°C, add 1.1 mol of p-toluenesulfonyl chloride in 2.5 L of tetrahydrofuran at a rate of 50 mL / min, return to room temperature and continue stirring for 22 hours, concentrate under reduced pressure and pass through column chromatography to obtain compound A; S2, 1 mol of compound A in step S1, 0.45 mol of 1,3-benzenedimethanol and 2 L of anhydrous methanol were mixed and stirred, 230 g of dilute sulfuric acid with a mass concentration of 47% was added, the temperature was raised to 65° C. and the mixture was stirred at a constant temperature for 10 h to obtain compound B; S3, 2.1 mol of magnesium metal and 7 L of anhydrous methanol were mixed, 1 mol of compound B in step S2 was added, and the mixture was stirred at room temperature for 7 h. After filtering, the filtrate was concentrated under reduced pressure to obtain compound C; S4, dissolving 2.1 mol of maleic anhydride in 1.5 L of dichloromethane, adding 226 g of dilute sulfuric acid with a mass concentration of 47% and heating to 37°C, adding 1 mol of compound C in step S3 in 1 L of dichloromethane dilution dropwise thereto, and continuing to stir at a constant temperature for 10 h after the addition is complete. After the reaction is completed, the temperature is lowered to 27°C, concentrated and dried under reduced pressure, and subjected to column chromatography to obtain a functional monomer; S5, add 1 mol of the functional monomer in step S4 to 6 L of deionized water, add 0.3 g of BC20 dispersant and 0.3 g of diisopropylbenzene peroxide, raise the temperature to 47°C, introduce N2 protective gas to replace the air in the reactor, and then introduce 5 mol of vinyl chloride gas, stir at a constant temperature for 5 h, filter after the reaction is completed, and obtain a modified polyvinyl chloride precursor; S6. Add 700 g of the modified polyvinyl chloride precursor in step S5 to 7 L of anhydrous ethanol, add 900 g of lanthanum nitrate in 10 L of anhydrous ethanol dilution thereto at a rate of 100 mL / min, then adjust the system pH to 6 with ammonia water, stir at room temperature for 4 h, let stand and then centrifuge and filter, wash with anhydrous ethanol and dry to obtain modified polyvinyl chloride.

[0049] Preparation Example 4 The preparation method of modified polyvinyl chloride has the same specific implementation as that of Preparation Example 3, except that the addition amount of 1,3-benzenedimethanol is 1 mol.

[0050] Preparation Example 5 The preparation method of modified polyvinyl chloride is the same as that of Preparation Example 3, except that an equal molar amount of glutaric acid is used instead of maleic anhydride.

[0051] Preparation Example 6 The preparation method of modified polyvinyl chloride is the same as that of Preparation Example 3, except that the added amount of the functional monomer is 3 mol.

[0052] Example 1 See also Figure 1 A highly weather-resistant flexible fabric membrane material, the flexible fabric membrane material comprises seven membrane layers, which, from top to bottom, comprise a polyvinylidene fluoride coating layer 1, a polyvinyl chloride layer 2, an adhesive layer 3, a base fabric layer 4, an adhesive layer 3, a polyvinyl chloride layer 2 and an acrylic treatment layer 5; The polyvinyl chloride layer 2 comprises the following raw materials by weight: 85 parts of modified polyvinyl chloride, 46 parts of diisooctyl adipate, 3 parts of polyethylene wax and 11 parts of nano titanium dioxide; The modified polyvinyl chloride is prepared by Preparation Example 3; The method for preparing the highly weather-resistant flexible fabric membrane material of this embodiment comprises the following steps: A 25 μm thick adhesive layer 3 is coated on the upper and lower surfaces of a 550 μm thick base fabric layer 4, and then a 230 μm thick polyvinyl chloride layer 2 is coated on the surface of the adhesive layer 3, and hot pressed at 145°C for 4 minutes to form, and then an acrylic treatment layer 5 with a thickness of 75 μm is coated on the lower polyvinyl chloride layer 2, and dried at 65°C for 15 minutes to form, and a 30 μm thick polyvinylidene fluoride coating layer 1 is coated on the upper polyvinyl chloride layer 2, and dried at 70°C for 25 minutes to obtain a highly weather-resistant flexible fabric membrane material.

[0053] Example 2 A highly weather-resistant flexible fabric membrane material, the flexible fabric membrane material comprises seven membrane layers, which, from top to bottom, sequentially comprise a polyvinylidene fluoride coating layer 1, a polyvinyl chloride layer 2, an adhesive layer 3, a base fabric layer 4, an adhesive layer 3, a polyvinyl chloride layer 2 and an acrylic treatment layer 5; The polyvinyl chloride layer 2 comprises the following raw materials by weight: 80 parts of modified polyvinyl chloride, 45 parts of diisooctyl adipate, 2 parts of polyethylene wax and 10 parts of nano titanium dioxide; The modified polyvinyl chloride is prepared by Preparation Example 3; The method for preparing the highly weather-resistant flexible fabric membrane material of this embodiment comprises the following steps: A 20 μm thick adhesive layer 3 is coated on the upper and lower surfaces of a 500 μm thick base fabric layer 4, and then a 200 μm thick polyvinyl chloride layer 2 is coated on the surface of the adhesive layer 3, and hot pressed at 140°C for 5 minutes to form, and then an acrylic treatment layer 5 with a thickness of 70 μm is coated on the lower polyvinyl chloride layer 2, and dried at 60°C for 20 minutes to form, and a 20 μm thick polyvinylidene fluoride coating layer 1 is coated on the upper polyvinyl chloride layer 2, and dried at 65°C for 30 minutes to obtain a highly weather-resistant flexible fabric membrane material.

[0054] Example 3 A highly weather-resistant flexible fabric membrane material, the flexible fabric membrane material comprises seven membrane layers, which, from top to bottom, sequentially comprise a polyvinylidene fluoride coating layer 1, a polyvinyl chloride layer 2, an adhesive layer 3, a base fabric layer 4, an adhesive layer 3, a polyvinyl chloride layer 2 and an acrylic treatment layer 5; The polyvinyl chloride layer 2 comprises the following raw materials by weight: 80 parts of modified polyvinyl chloride, 45 parts of diisooctyl adipate, 2 parts of polyethylene wax and 12 parts of nano titanium dioxide; The modified polyvinyl chloride is prepared by Preparation Example 3; The method for preparing the highly weather-resistant flexible fabric membrane material of this embodiment comprises the following steps: A 30 μm thick adhesive layer 3 is coated on the upper and lower surfaces of a 600 μm thick base fabric layer 4, and then a 250 μm thick polyvinyl chloride layer 2 is coated on the surface of the adhesive layer 3, and hot pressed at 150°C for 3 minutes to form, and then an 80 μm thick acrylic treatment layer 5 is coated on the lower polyvinyl chloride layer 2, and dried at 70°C for 10 minutes to form, and a 40 μm thick polyvinylidene fluoride coating layer 1 is coated on the upper polyvinyl chloride layer 2, and dried at 75°C for 20 minutes to obtain a highly weather-resistant flexible fabric membrane material.

[0055] Example 4 A highly weather-resistant flexible fabric membrane material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified polyvinyl chloride is prepared by Preparation Example 4.

[0056] Example 5 A highly weather-resistant flexible fabric membrane material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified polyvinyl chloride is prepared by Preparation Example 5.

[0057] Example 6 A highly weather-resistant flexible fabric membrane material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified polyvinyl chloride is prepared by Preparation Example 6.

[0058] Comparative Example 1 See also Figure 1 , and an equal amount of commercially available polyvinyl chloride is used instead of modified polyvinyl chloride.

[0059] Performance Testing: (1) Tensile strength test: Tested according to the method of GB / T1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets"; (2) Film adhesion: According to the GB / T38464-2020 test method, the flexible fabric film material was rubbed 20,000 times and its separation was observed; (3) Infrared reflectivity and UV blocking rate: tested using Shimadzu UV-3600i Plus UV-visible near-infrared spectrophotometer; (4) Aging resistance test: The flexible fabric membrane is placed in an environment with a temperature of 60°C, a light temperature of 40°C, and an ultraviolet wavelength of 400 nm for 144 h, and then its tensile strength after aging is tested according to method (1); (5) Weathering test: The flexible fabric membrane was placed in -60℃ and 100℃ environments for 2 hours, and its tensile strength was tested.

[0060] The flexible fabric membranes of the embodiments and comparative examples were tested according to the above test method. The results are shown in Table 1.

[0061] Table 1

[0062] According to the data in Table 1, the flexible fabric membranes of Examples 1 to 3 have good tensile strength, weather resistance, excellent anti-ultraviolet infrared performance and anti-aging performance, and at the same time, the adhesion of the coating is good, and there is no obvious stratification phenomenon under high rubbing; in Example 4, due to the change in the molar ratio of compound A and 1,3-benzenedimethanol, the modified polyvinyl chloride does not contain a cross-linked network structure, which leads to a decrease in the tensile strength of the flexible fabric membrane; in Example 5, due to the use of equimolar glutaric acid instead of maleic anhydride, the modified polyvinyl chloride does not contain a cross-linked network structure, which leads to an increase in the tensile strength of the flexible fabric membrane. The degree of tensile strength, high temperature resistance and flexibility of the flexible fabric membrane material are weakened due to the use of equal mass parts of commercially available polyvinyl chloride instead of modified polyvinyl chloride in Comparative Example 1. At the same time, since it cannot form stable hydrogen bonds with the polyvinylidene fluoride coating layer 1, the bonding performance between the film layers is reduced, and stratification occurs after rubbing.

[0063] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A highly weather-resistant flexible fabric membrane material, It is characterized in that The flexible fabric membrane material comprises seven membrane layers, which, from top to bottom, include a polyvinylidene fluoride coating layer (1), a polyvinyl chloride layer (2), an adhesive layer (3), a base fabric layer (4), an adhesive layer (3), a polyvinyl chloride layer (2), and an acrylic treatment layer (5); The polyvinyl chloride layer (2) comprises the following raw materials in parts by weight: 80 to 90 parts of modified polyvinyl chloride, 45 to 47 parts of a plasticizer, 2 to 4 parts of a lubricant, and 10 to 12 parts of nano titanium dioxide.

2. A highly weather-resistant flexible fabric membrane material according to claim 1, It is characterized in that The polyvinylidene fluoride coating layer (1) comprises the following raw materials in parts by weight: 80-90 parts of modified polyvinylidene fluoride, 20-24 parts of titanium dioxide grafted modified aramid fiber, 10-14 parts of polymethyl methacrylate, 1-5 parts of inorganic filler, 30-40 parts of deionized water and 30-40 parts of anhydrous ethanol.

3. The highly weather-resistant flexible fabric membrane material according to claim 1, It is characterized in that The preparation method of the modified polyvinyl chloride comprises the following steps: S1. Mix 2-aminonicotinic acid and triethylamine in tetrahydrofuran, cool to -5~0°C, add p-toluenesulfonyl chloride in tetrahydrofuran dropwise, return to room temperature and continue stirring for 20~24h, concentrate under reduced pressure and pass through column chromatography to obtain compound A; S2, mixing compound A, 1,3-benzenedimethanol and anhydrous methanol in step S1, adding dilute sulfuric acid, heating to 60-70° C. and stirring at constant temperature for 8-12 hours to obtain compound B; S3, 0.45 g of magnesium metal and 15 ml of anhydrous methanol were mixed, 0.74 g of compound B in step S2 was added, and the mixture was stirred at room temperature for 6 to 8 hours. After filtering, the filtrate was concentrated under reduced pressure to obtain compound C; S4, dissolving maleic anhydride in dichloromethane, adding dilute sulfuric acid thereto and heating to 35-40°C, adding the dichloromethane dilution of compound C in step S3 dropwise thereto, and continuing to stir at a constant temperature for 8-12 hours after the addition is complete. After the reaction is completed, cool to room temperature, concentrate and dry under reduced pressure, and perform column chromatography to obtain a functional monomer; S5, adding the functional monomer in step S4 into deionized water, adding a dispersant and an initiator, heating to 45-50° C., introducing an inert protective gas to replace the air in the reactor, and then introducing vinyl chloride gas, stirring at a constant temperature for 4-6 hours, filtering after the reaction is completed, and obtaining a modified polyvinyl chloride precursor; S6. Add the modified polyvinyl chloride precursor in step S5 into anhydrous ethanol, add a diluted anhydrous ethanol solution of lanthanum nitrate dropwise thereto, then adjust the system pH to 6-7 with aqueous ammonia, stir at room temperature for 4-5 hours, let stand, centrifuge and filter, wash and dry to obtain modified polyvinyl chloride.

4. A highly weather-resistant flexible fabric membrane material according to claim 3, It is characterized in that In step S2, the molar ratio of compound A to 1,3-benzenedimethanol is 1:(0.4-0.5).

5. The highly weather-resistant flexible fabric membrane material according to claim 3, It is characterized in that In step S4, the molar ratio of compound C to maleic anhydride is 1:(2-2.2).

6. The highly weather-resistant flexible fabric membrane material according to claim 3, It is characterized in that In step S5, the molar ratio of the functional monomer to the vinyl chloride gas is (0.1-0.3):

1.

7. The highly weather-resistant flexible fabric membrane material according to claim 1, It is characterized in that The adhesive layer (3) is acrylate.

8. The highly weather-resistant flexible fabric membrane material according to claim 1, It is characterized in that The acrylic treatment layer (5) comprises the following raw materials in parts by weight: 88 to 90 parts of polymethyl methacrylate, 8 to 10 parts of diisononyl phthalate, 1 to 2 parts of titanium dioxide, and 1 to 1.5 parts of a heat stabilizer.

9. A method for preparing the highly weather-resistant flexible fabric membrane material according to any one of claims 1 to 8, It is characterized in that The steps include: An adhesive layer (3) is coated on the upper and lower surfaces of the base fabric layer (4), and then a polyvinyl chloride layer (2) is coated on the surface of the adhesive layer (3), and hot pressing is performed at 140-150°C for 3-5 minutes to form the adhesive layer. Then, an acrylic treatment layer (5) is coated on the lower polyvinyl chloride layer (2), and the adhesive layer is dried at 60-70°C for 10-20 minutes to form the adhesive layer. Then, a polyvinylidene fluoride coating layer (1) is coated on the upper polyvinyl chloride layer (2), and the adhesive layer is dried at 65-75°C for 20-30 minutes to obtain a highly weather-resistant flexible fabric membrane material.

10. A method for preparing a highly weather-resistant flexible fabric membrane according to claim 9, It is characterized in that The polyvinylidene fluoride coating layer (1) has a thickness of 20 to 40 μm; the polyvinyl chloride layer (2) has a thickness of 200 to 250 μm; the adhesive layer (3) has a thickness of 20 to 30 μm; the base fabric layer (4) has a thickness of 500 to 600 μm; and the acrylic treatment layer (5) has a thickness of 70 to 80 μm.

Citation Information

Patent Citations

  • High-performance composite film and preparation method thereof

    CN118752874A