Preparation method of aluminum / copper foil adhesive tape for heater and aluminum / copper foil adhesive tape
Through the combined preparation method of hot melt adhesive and pressure sensitive adhesive, the problem of insufficient bonding strength of the existing aluminum/copper foil tape is solved, and high-strength, weather resistance and heat resistance aluminum/copper foil tape is achieved to ensure the heater Stable bonding to tape and long-term use.
Patent Information
- Application Number
- CN202411352775.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
AI Technical Summary
The bonding strength of the existing domestic smart toilet and refrigerator defrosting heaters is not high, and the heat resistance and boiling resistance are poor, resulting in the bonding of the aluminum/copper foil and the heating wires being not firmly combined and insufficient peeling strength.
Using a combination of hot melt adhesive and pressure-sensitive adhesive, a hot melt adhesive film layer is formed on an aluminum/copper foil substrate by hot melt adhesive, and a pressure-sensitive adhesive is applied below it to form a pressure-sensitive adhesive film layer. Combined with baking processing, improve bonding strength and weather resistance.
High-strength bonding between the heater and the aluminum/copper foil tape is achieved, and weather resistance and heat resistance are improved, making the heater and tape difficult to separate and extend the service life.
Smart Images

Figure CN119081566A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum / copper foil tapes, and in particular to a preparation method of an aluminum / copper foil tape for a heater and the aluminum / copper foil tape. Background Art
[0002] As the market's requirements for the performance of aluminum / copper foil tapes for smart toilets and refrigerator defrost heaters become increasingly higher, the performance of existing domestically produced aluminum / copper foil tapes for smart toilets and refrigerator defrost heaters is slightly insufficient. The bonding strength between traditional heating aluminum / copper foil heating wires and aluminum / copper foil is not high, and the heat resistance and water boiling resistance are poor, resulting in weak bonding between the aluminum / copper foil and the heating wire, and the peeling strength does not meet customer requirements. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing an aluminum / copper foil tape for a heater, wherein the prepared aluminum / copper foil tape has good adhesive properties and is not easily separated from the heater.
[0004] The invention also provides an aluminum / copper foil tape.
[0005] According to the first aspect of the present invention, a method for preparing an aluminum / copper foil tape for a heater comprises: a hot melt adhesive preparation process, a pressure sensitive adhesive preparation process and a tape preparation process;
[0006] Among them, the hot melt adhesive is prepared through the hot melt adhesive preparation process, and the pressure sensitive adhesive is prepared through the tape preparation process;
[0007] The tape preparation process includes the following steps:
[0008] Preparing a substrate, wherein the substrate is aluminum foil or copper foil;
[0009] a hot melt adhesive coating step, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate to form a hot melt adhesive coating on the upper end surface of the substrate, and baking the hot melt adhesive coating to form a hot melt adhesive film layer;
[0010] A pressure-sensitive adhesive coating step is to coat the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step onto the lower end surface of the substrate to form a pressure-sensitive adhesive coating on the lower end surface of the substrate, bake the pressure-sensitive adhesive coating to form a pressure-sensitive adhesive film layer, and set a release paper on the lower end surface of the pressure-sensitive adhesive film layer.
[0011] According to the preparation method of the aluminum / copper foil tape for a heater according to the embodiment of the present invention, there are at least the following beneficial effects: the hot-melt adhesive film layer is used to be bonded to the heater, and the pressure-sensitive adhesive film layer is used to be bonded to the attachment after the release paper is removed. Since the hot-melt adhesive film layer is prefabricated on the end surface of the aluminum foil or copper foil and is processed by baking, it has good bonding strength with the aluminum foil or copper foil. When used, after the heater and the hot-melt adhesive film layer are bonded together, the bonding strength between the heater and the hot-melt adhesive film layer is high, it is not easy to separate, and it has good weather resistance and heat resistance.
[0012] According to some embodiments of the present invention, the thickness of the substrate is 15-60 μm.
[0013] According to some embodiments of the present invention, the dyne value of the substrate is greater than 52 dynes.
[0014] According to some embodiments of the present invention, in the hot melt adhesive coating process, the baking temperature when baking the hot melt adhesive coating is 110-130°C.
[0015] According to some embodiments of the present invention, in the hot melt adhesive coating process, the thickness of the hot melt adhesive coating is 1-20 μm.
[0016] According to some embodiments of the present invention, in the hot melt adhesive coating process, the coating speed of the hot melt adhesive is 15-20 m / min.
[0017] According to some embodiments of the present invention, the hot melt adhesive in the hot melt adhesive preparation process includes the following components by mass: 60-90 parts of polyurethane resin, 10-40 parts of epoxy resin, 10-30 parts of solvent, 0.01-0.5 parts of leveling agent, and 0.01-0.05 parts of curing agent.
[0018] According to some embodiments of the present invention, the hot melt adhesive preparation process includes:
[0019] Step 1.1, put polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly;
[0020] Step 1.2: Add curing agent into the stirring kettle and continue stirring until hot melt adhesive is obtained after stirring evenly.
[0021] According to some embodiments of the present invention, in the hot melt adhesive preparation process, the hot melt adhesive includes 1-2 parts by mass of a tackifier, and the tackifier is added into the stirring kettle in step 1.1 or in step 1.2.
[0022] According to some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the baking temperature when baking the pressure-sensitive adhesive coating is 100-110°C.
[0023] According to some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the thickness of the pressure-sensitive adhesive coating is 10-70 μm.
[0024] According to some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the pressure-sensitive adhesive coating speed is 15-20 m / min.
[0025] According to some embodiments of the present invention, the pressure-sensitive adhesive in the pressure-sensitive adhesive preparation process includes the following components by mass: 50-80 parts of acrylic resin, 1-5 parts of tackifying resin, 1-3 parts of modifier, 1-10 parts of curing agent, and 10-30 parts of solvent.
[0026] According to the aluminum / copper foil tape of the second embodiment of the present invention, the aluminum / copper foil tape is made by the preparation method of the aluminum / copper foil tape for a heater described in any of the above embodiments.
[0027] The aluminum / copper foil tape according to the embodiment of the present invention has at least the following beneficial effects: the obtained aluminum / copper foil tape has high bonding strength, is not easy to separate, and has good weather resistance, heat resistance and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0029] Figure 1 Schematic diagram of the structure of the aluminum / copper foil tape according to an embodiment of the present invention.
[0030] Reference numerals:
[0031] A substrate 100 , a hot melt adhesive film layer 200 , a pressure sensitive adhesive film layer 300 , and a release paper 400 . DETAILED DESCRIPTION
[0032] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0033] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, front, back, left, right, etc., and orientations or positional relationships indicated are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0034] In the description of the present invention, if there is a description of first and second, it is only for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0035] In the description of the present invention, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention based on the specific content of the technical solution.
[0036] Reference below Figure 1 An aluminum / copper foil tape according to an embodiment of the present invention is described.
[0037] The method for preparing the aluminum / copper foil tape for a heater according to an embodiment of the present invention comprises: a hot melt adhesive preparation process, a pressure sensitive adhesive preparation process and a tape preparation process;
[0038] Among them, the hot melt adhesive is prepared through the hot melt adhesive preparation process, and the pressure sensitive adhesive is prepared through the tape preparation process;
[0039] The tape preparation process includes the following steps:
[0040] Prepare a substrate 100, the substrate 100 is aluminum foil or copper foil;
[0041] A hot melt adhesive coating step, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate 100 to form a hot melt adhesive coating on the upper end surface of the substrate 100, and baking the hot melt adhesive coating to form a hot melt adhesive film layer 200;
[0042] In the pressure-sensitive adhesive coating step, the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step is coated on the lower end surface of the substrate 100 to form a pressure-sensitive adhesive coating on the lower end surface of the substrate 100, and the pressure-sensitive adhesive coating is baked to form a pressure-sensitive adhesive film layer 300, and a release paper 400 is set on the lower end surface of the pressure-sensitive adhesive film layer 300.
[0043] The hot-melt adhesive film layer 200 is used to be bonded to the heater, and after the release paper 400 is removed, the pressure-sensitive adhesive film layer 300 is used to be bonded to the attachment. Since the hot-melt adhesive film layer 200 is prefabricated on the end surface of the aluminum foil or copper foil and is processed by baking, it has good bonding strength with the aluminum foil or copper foil. When used, after the heater and the hot-melt adhesive film layer 200 are bonded together, the heater and the hot-melt adhesive film layer 200 have high bonding strength, are not easy to separate, and have good weather resistance and heat resistance.
[0044] Specifically, the heater is generally a heating wire, a heating sheet, a heating film, etc., which can be directly attached to the hot melt adhesive film layer 200, and through heating means, the two have a higher bonding strength.
[0045] When the device is in use, the heater can heat the hot melt adhesive film layer 200 at a low temperature, so that the heater and the hot melt adhesive film layer 200 can maintain good bonding performance for a long time, have a long service life, and have good durability.
[0046] Meanwhile, the pressure-sensitive adhesive film layer 300 is formed by baking the pressure-sensitive adhesive coating and has a high bonding strength.
[0047] In some embodiments of the present invention, the thickness of the substrate 100 is 15-60 μm, so that the prepared aluminum / copper foil tape has a certain structural strength to meet the requirements of mounting.
[0048] In some embodiments of the present invention, the dyne value of the substrate 100 is greater than 52 dynes, so that the substrate 100 has better adhesive adhesion and higher adhesive strength.
[0049] Specifically, the dyne value of the substrate 100 is 55 dynes, 58 dynes, 60 dynes, etc., and can be used to bond aluminum / copper foil tapes with relatively high bonding strength.
[0050] In some embodiments of the present invention, in the hot melt adhesive coating process, the baking temperature when baking the hot melt adhesive coating is 110-130° C. to form a hot melt adhesive film layer 200 with a better bonding effect.
[0051] Specifically, the hot melt adhesive coating can be baked at a temperature of 110° C., 120° C., or 130° C. to form a hot melt adhesive film layer 200 with good bonding performance.
[0052] In some embodiments of the present invention, in the hot melt adhesive coating process, the thickness of the hot melt adhesive coating is 1-20 μm, so that the formed hot melt adhesive film layer 200 has a certain thickness and has a high bonding strength with the heater.
[0053] Specifically, the hot melt adhesive coating having a thickness of 1 μm, 5 μm, 10 μm, 15 μm, and 20 μm can all meet the bonding requirements of the heater and have good weather resistance and heat resistance.
[0054] In some embodiments of the present invention, in the hot melt adhesive coating process, the coating speed of the hot melt adhesive is 15-20 m / min, so that the hot melt adhesive is coated evenly and the thickness remains roughly consistent.
[0055] In some embodiments of the present invention, the hot melt adhesive in the hot melt adhesive preparation process includes the following components by mass: 60-90 parts of polyurethane resin, 10-40 parts of epoxy resin, 10-30 parts of solvent, 0.01-0.5 parts of leveling agent, and 0.01-0.05 parts of curing agent. The prepared hot melt adhesive has good weather resistance, heat resistance and durability.
[0056] In some embodiments of the present invention, the hot melt adhesive preparation process includes:
[0057] Step 1.1, put polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly;
[0058] Step 1.2: Add curing agent into the stirring kettle and continue stirring until hot melt adhesive is obtained after stirring evenly.
[0059] In some embodiments of the present invention, the hot melt adhesive in the hot melt adhesive preparation process includes 1-2 parts by mass of a tackifier, and the tackifier is added into the stirring kettle in step 1.1 or in step 1.2 to further enhance the bonding performance of the hot melt adhesive.
[0060] In some embodiments of the present invention, the polyurethane resin is any one of L3900, P3850, and P5836.
[0061] In some embodiments of the present invention, the epoxy resin is any one of SM3000, 901, and 7160.
[0062] In some embodiments of the present invention, the leveling agent is any one of LD9310 and BYK316.
[0063] In some embodiments of the present invention, the curing agent is any one of N3300 and DMP30.
[0064] In some embodiments of the present invention, the adhesion promoter is any one of resins, silane coupling agents, titanate coupling agents, and organic polymer compounds, and the adhesion promoter can be used to improve the adhesion between the film layer and the substrate or the heater.
[0065] In some embodiments of the present invention, the solvent is any one of ethyl acetate, xylene, toluene, and butanone.
[0066] In some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the baking temperature when baking the pressure-sensitive adhesive coating is 100-110° C. to form a pressure-sensitive adhesive film layer 300 with better bonding effect.
[0067] Specifically, the pressure-sensitive adhesive film layer 300 with good adhesive properties can be formed when the baking temperature of the pressure-sensitive adhesive coating is 100° C., 105° C., or 110° C.
[0068] In some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the thickness of the pressure-sensitive adhesive coating is 10-70 μm, so that the formed pressure-sensitive adhesive film layer 300 has a certain thickness and has a high bonding strength with the attached object.
[0069] Specifically, the thickness of the pressure-sensitive adhesive coating is 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, and 70 μm, which can meet the bonding requirements of the aluminum / copper foil tape and have bonding properties.
[0070] In some embodiments of the present invention, in the pressure-sensitive adhesive coating process, the pressure-sensitive adhesive coating speed is 15-20 m / min, so that the hot melt adhesive is coated evenly and the thickness remains roughly consistent.
[0071] In some embodiments of the present invention, the pressure-sensitive adhesive in the pressure-sensitive adhesive preparation process includes the following components in parts by mass: 50-80 parts of acrylic resin, 1-5 parts of tackifying resin, 1-3 parts of modifier, 1-10 parts of curing agent, and 10-30 parts of solvent. The prepared pressure-sensitive adhesive has good bonding properties, so that it has good bonding strength with the attached object and is not easy to separate.
[0072] Specifically, acrylic resin, modifier and solvent are put into a stirring kettle and stirred evenly, and then tackifying resin and curing agent are added into the stirring kettle and stirred continuously, and the pressure-sensitive adhesive is obtained after stirring evenly.
[0073] In some embodiments of the present invention, the acrylic resin raw material is any one or more of natural rubber, synthetic rubber and acrylate.
[0074] In some embodiments of the present invention, the solvent is any one of ethyl acetate, xylene, toluene, and butanone.
[0075] According to the aluminum / copper foil tape of the second aspect embodiment of the present invention, the aluminum / copper foil tape is made by the preparation method of the aluminum / copper foil tape for a heater of any of the above embodiments. The prepared aluminum / copper foil tape has high bonding strength, is not easy to fall off, and has good weather resistance, heat resistance and durability.
[0076] Specifically, Figure 1 As shown, the aluminum / copper foil tape includes a hot melt adhesive film layer 200, a substrate 100, a pressure sensitive adhesive film layer 300, and a release paper 400 from top to bottom.
[0077] The aluminum / copper foil tape prepared by the above preparation method has the advantages of good weather resistance, heat resistance, high and low temperature impact resistance, and adhesion performance compared with traditional products. The bonding strength between the traditional heating aluminum foil and the heating wire is not high, and the heat resistance and boiling resistance are poor, resulting in the aluminum foil and the heating wire not being firmly bonded, and the peeling strength does not meet customer requirements, such as: the heating wire and the aluminum foil fall off after the boiling resistance test, the heating wire and the aluminum foil fall off after the heat resistance test, and the heating wire and the aluminum foil fall off after the hot and cold shock test. The aluminum / copper foil tape prepared by the above preparation method can directly tear the aluminum / copper foil when the heating wire and the aluminum / copper foil are peeled off after the above performance tests, proving that it can maintain a high bonding strength in the above tests.
[0078] In order to better understand the above technical solution, the above technical solution will be described in detail below in combination with specific implementation methods.
[0079] Embodiment 1
[0080] Aluminum foil tape is prepared by the following process:
[0081] S1: preparing a substrate 100, the substrate 100 is an aluminum foil with a thickness of 30 μm and a dyne value of 55 dynes;
[0082] S2: Prepare hot melt adhesive. Prepare the following components by mass: 80 parts of polyurethane resin, 15 parts of epoxy resin, 25 parts of solvent, 0.4 parts of leveling agent, 0.02 parts of curing agent, and 1 part of tackifier. Put the polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly. Then add the curing agent and tackifier into the stirring kettle and continue stirring to obtain the hot melt adhesive.
[0083] S3, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate 100 at a coating speed of 18 m / min, forming a hot melt adhesive coating on the upper end surface of the substrate 100, the hot melt adhesive coating having a thickness of 10 μm, baking the hot melt adhesive coating at a baking temperature of 110° C., so that the hot melt adhesive coating forms a hot melt adhesive film layer 200;
[0084] S4, prepare a pressure-sensitive adhesive, prepare the following components by mass: 50 parts of acrylic resin, 4 parts of tackifying resin, 3 parts of modifier, 2 parts of curing agent, 250 parts of solvent, put the acrylic resin, modifier, and solvent into a stirring kettle and stir evenly, then add the tackifying resin and curing agent into the stirring kettle and continue stirring, and stir evenly to obtain a pressure-sensitive adhesive;
[0085] S4, coating the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step onto the lower end surface of the substrate 100 at a coating speed of 18 m / min, forming a pressure-sensitive adhesive coating on the lower end surface of the substrate 100, the thickness of the pressure-sensitive adhesive coating being 60 μm, baking the pressure-sensitive adhesive coating at a baking temperature of 100° C., so that the pressure-sensitive adhesive coating forms a pressure-sensitive adhesive film layer 300;
[0086] S5 . Dispose a release paper 400 on the lower end surface of the pressure-sensitive adhesive film layer 300 .
[0087] The aluminum foil tape can be produced, which has the advantages of good weather resistance, heat resistance, high and low temperature impact resistance, adhesion performance, etc. In the high and low temperature impact test, heat resistance test, humidity resistance test, boiling water resistance test, low temperature resistance test, and water resistance test, a higher peeling force can be obtained, and there is no peeling phenomenon of the heater / wire.
[0088] Embodiment 2:
[0089] Aluminum foil tape is prepared by the following process:
[0090] S1: preparing a substrate 100, the substrate 100 is an aluminum foil, the thickness is 60 μm, and the dyne value is 60 dynes;
[0091] S2: Prepare hot melt adhesive. Prepare the following components by mass: 90 parts of polyurethane resin, 40 parts of epoxy resin, 15 parts of solvent, 0.1 parts of leveling agent, 0.02 parts of curing agent, and 2 parts of tackifier. Put the polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly. Then add the curing agent and tackifier into the stirring kettle and continue stirring to obtain the hot melt adhesive.
[0092] S3, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate 100 at a coating speed of 20 m / min, forming a hot melt adhesive coating on the upper end surface of the substrate 100, the hot melt adhesive coating having a thickness of 20 μm, baking the hot melt adhesive coating at a baking temperature of 130° C., so that the hot melt adhesive coating forms a hot melt adhesive film layer 200;
[0093] S4, prepare a pressure-sensitive adhesive, prepare the following components by mass: 55 parts of acrylic resin, 5 parts of tackifying resin, 3 parts of modifier, 10 parts of curing agent, and 30 parts of solvent, put the acrylic resin, modifier, and solvent into a stirring kettle and stir evenly, then add the tackifying resin and curing agent into the stirring kettle and continue stirring, and stir evenly to obtain a pressure-sensitive adhesive;
[0094] S4, coating the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step onto the lower end surface of the substrate 100 at a coating speed of 20 m / min, forming a pressure-sensitive adhesive coating on the lower end surface of the substrate 100, the pressure-sensitive adhesive coating having a thickness of 40 μm, baking the pressure-sensitive adhesive coating at a baking temperature of 110° C., so that the pressure-sensitive adhesive coating forms a pressure-sensitive adhesive film layer 300;
[0095] S5 . Dispose a release paper 400 on the lower end surface of the pressure-sensitive adhesive film layer 300 .
[0096] The aluminum foil tape can be produced, which has the advantages of good weather resistance, heat resistance, high and low temperature impact resistance, adhesion performance, etc. In the high and low temperature impact test, heat resistance test, humidity resistance test, boiling water resistance test, low temperature resistance test, and water resistance test, a higher peeling force can be obtained, and there is no peeling phenomenon of the heater / wire.
[0097] Embodiment 3
[0098] Copper foil tape is prepared by the following process:
[0099] S1: preparing a substrate 100, the substrate 100 is a copper foil with a thickness of 18 μm and a dyne value of 57 dynes;
[0100] S2: Prepare hot melt adhesive. Prepare the following components by mass: 65 parts of polyurethane resin, 15 parts of epoxy resin, 10 parts of solvent, 0.02 parts of leveling agent, 0.05 parts of curing agent, and 2 parts of tackifier. Put the polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly. Then add the curing agent and tackifier into the stirring kettle and continue stirring to obtain the hot melt adhesive.
[0101] S3, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate 100 at a coating speed of 15 m / min, forming a hot melt adhesive coating on the upper end surface of the substrate 100, the hot melt adhesive coating having a thickness of 5 μm, baking the hot melt adhesive coating at a baking temperature of 120° C., so that the hot melt adhesive coating forms a hot melt adhesive film layer 200;
[0102] S4, prepare a pressure-sensitive adhesive, prepare the following components by mass: 50 parts of acrylic resin, 5 parts of tackifying resin, 1 part of modifier, 8 parts of curing agent, and 10 parts of solvent, put the acrylic resin, modifier, and solvent into a stirring kettle and stir evenly, then add the tackifying resin and curing agent into the stirring kettle and continue stirring, and stir evenly to obtain a pressure-sensitive adhesive;
[0103] S4, coating the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step onto the lower end surface of the substrate 100 at a coating speed of 15 m / min, forming a pressure-sensitive adhesive coating on the lower end surface of the substrate 100, the pressure-sensitive adhesive coating having a thickness of 70 μm, and baking the pressure-sensitive adhesive coating at a baking temperature of 105° C. so that the pressure-sensitive adhesive coating forms a pressure-sensitive adhesive film layer 300;
[0104] S5 . Dispose a release paper 400 on the lower end surface of the pressure-sensitive adhesive film layer 300 .
[0105] The copper foil tape can be produced, which has the advantages of good weather resistance, heat resistance, high and low temperature impact resistance, adhesion performance, etc. In the high and low temperature impact test, heat resistance test, humidity resistance test, boiling water resistance test, low temperature resistance test, and water resistance test, a higher peeling force can be obtained, and there is no peeling phenomenon on the heater / wire.
[0106] Of course, the invention is not limited to the above-mentioned embodiments, and those skilled in the art may make equivalent modifications or substitutions without violating the spirit of the invention, and these equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for preparing aluminum / copper foil tape for heater, It is characterized in that include: Hot melt adhesive preparation process, pressure sensitive adhesive preparation process and adhesive tape preparation process; Among them, the hot melt adhesive is prepared through the hot melt adhesive preparation process, and the pressure sensitive adhesive is prepared through the tape preparation process; The tape preparation process includes the following steps: Preparing a substrate, wherein the substrate is aluminum foil or copper foil; a hot melt adhesive coating step, coating the hot melt adhesive prepared in the hot melt adhesive preparation step onto the upper end surface of the substrate to form a hot melt adhesive coating on the upper end surface of the substrate, and baking the hot melt adhesive coating to form a hot melt adhesive film layer; A pressure-sensitive adhesive coating step is to coat the pressure-sensitive adhesive prepared in the pressure-sensitive adhesive preparation step onto the lower end surface of the substrate to form a pressure-sensitive adhesive coating on the lower end surface of the substrate, bake the pressure-sensitive adhesive coating to form a pressure-sensitive adhesive film layer, and set a release paper on the lower end surface of the pressure-sensitive adhesive film layer.
2. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that The substrate has a dyne value greater than 52 dynes.
3. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that In the hot melt adhesive coating process, the baking temperature when baking the hot melt adhesive coating is 110-130°C.
4. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that In the hot melt adhesive coating process, the thickness of the hot melt adhesive coating is 1-20 μm.
5. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that In the hot melt adhesive preparation process, the hot melt adhesive comprises the following components by weight: 60-90 parts of polyurethane resin, 10-40 parts of epoxy resin, 10-30 parts of solvent, 0.01-0.5 parts of leveling agent, and 0.01-0.05 parts of curing agent.
6. The method for preparing the aluminum / copper foil tape for heater according to claim 7, It is characterized in that The hot melt adhesive preparation process comprises: Step 1.1, put polyurethane resin, epoxy resin, solvent and leveling agent into a stirring kettle and stir evenly; Step 1.2: Add curing agent into the stirring kettle and continue stirring until hot melt adhesive is obtained after stirring evenly.
7. The method for preparing the aluminum / copper foil tape for heater according to claim 8, It is characterized in that In the hot melt adhesive preparation process, the hot melt adhesive includes 1-2 parts by mass of a tackifier, and the tackifier is added into the stirring kettle in step 1.1 or in step 1.
2.
8. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that In the pressure-sensitive adhesive coating process, the baking temperature when baking the pressure-sensitive adhesive coating is 100-110°C.
9. The method for preparing the aluminum / copper foil tape for heater according to claim 1, It is characterized in that The pressure-sensitive adhesive in the pressure-sensitive adhesive preparation process comprises the following components by mass: 50-80 parts of acrylic resin, 1-5 parts of tackifying resin, 1-3 parts of modifier, 1-10 parts of curing agent, and 10-30 parts of solvent.
10. Aluminum / copper foil tape, Features: The aluminum / copper foil tape is made by the preparation method of the aluminum / copper foil tape for a heater according to any one of claims 1 to 9.