Hot melt adhesive composition and application thereof

By using hot melt adhesive composition coating and sand blasting methods, the problem of complex and poor support points of the protection silicon carbide coating in the prior art is solved, and better adhesive and anti-oxidation properties are achieved, and operation is simplified. And improve the thermal shock performance of the product.

CN119081583APending Publication Date: 2024-12-06湖南德智新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411376846.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art uses methods when protecting the support points of the silicon carbide coating, and the methods used are complicated and have poor results. After vacuum mud and epoxy resin are filled, they are easily washed away by silicon carbide sand or lead to impurities on the coating surface, affecting the appearance of the product.

Method used

Using hot melt adhesive compositions, including high molecular weight matrix resins, petroleum-based plasticizers and ester plasticizers, protect the support points of the silicon carbide coating through hot melt adhesive coating and sand blasting methods, improve adhesion and resistance. Oxidation properties.

Benefits of technology

The hot melt adhesive composition provides better adhesive performance and protection effect, avoiding the hot melt adhesive falling off during sand blasting, improving the thermal shock and oxidation resistance of silicon carbide products, simplifying the operation process and improving processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070205500000151
    Figure BDA0005070205500000151
  • Figure BDA0005070205500000161
    Figure BDA0005070205500000161
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor material preparation, and provides a hot melt adhesive composition and application thereof. The hot melt adhesive composition is prepared from the following components in parts by weight: 60 to 90 parts of matrix resin, 12 to 20 parts of tackifier, 0.1 to 0.5 part of plasticizer and 0.1 to 2 parts of antioxidant, the matrix resin is macromolecular resin with the molecular weight of 50,000 to 100,000 g / mol; the plasticizer comprises a petroleum-based plasticizer and an ester plasticizer. Under the combined action of the matrix resin, the tackifier, the plasticizer, the antioxidant and other assistants, the hot melt adhesive prepared from the hot melt adhesive composition has good bonding performance and can be better combined with a weak area of a supporting point of a matrix silicon carbide coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor material preparation, and in particular to a hot melt adhesive composition and application thereof. Background Art

[0002] When CVD vapor deposition grows silicon carbide coating products on the graphite surface, when there is turbulent airflow locally in the deposition furnace, it will leave different colors on the product surface; or when the coating collapses on the accessories in the furnace, it is easy to form slag and particles on the coating surface. After deposition, the product surface needs to be polished, leaving polishing marks on the product surface. For these two situations, the product surface needs to be sandblasted. Sandblasting is to use the high-speed impact of silicon carbide sand to scour and polish the product surface, so that the color of the product surface is more uniform.

[0003] To grow silicon carbide coating on the graphite surface by CVD vapor deposition, the graphite needs to be supported and then deposited. After deposition, supporting points will be left at the supporting positions, and the coating at these supporting positions is relatively weak. During the sandblasting process, it is easy to be damaged by the high-speed impact of silicon carbide sand and expose the graphite substrate. Therefore, it is very necessary to protect the supporting points before sandblasting. Summary of the invention

[0004] In the prior art, some means of protecting support points take a long time and are complicated to operate, and the improvement effect is not good. For example, in some prior art, vacuum mud is used to fill the support points. Vacuum mud is a plastic putty made by mixing refined petroleum grease and high mountain residual soil. After the vacuum mud is used to fill the support points, due to the low hardness of the vacuum mud, the vacuum mud is easily washed away by silicon carbide sand during the sandblasting process; and after the sandblasting, the vacuum mud remaining inside the support point is difficult to remove. For example, in other prior art, epoxy resin is used for filling. After the epoxy resin is used to fill the support points, the epoxy resin AB glue has a long curing time at room temperature and is more viscous. It usually needs to be placed in an oven and heated for 2-3 hours to accelerate curing, and the removal of the epoxy resin glue requires the help of pickling. The pickling process is also prone to cause impurities on the surface of the coating to react with the acidic solution, resulting in poor appearance.

[0005] The purpose of the present invention is to overcome the above problems existing in the prior art, and to provide a hot melt adhesive composition, and the use of the hot melt adhesive prepared by the hot melt adhesive composition in the method for sandblasting the surface of a silicon carbide coating, and the method for sandblasting the surface of a silicon carbide coating. The matrix resin and auxiliary agents such as tackifiers, plasticizers and antioxidants work together to make the hot melt adhesive have better adhesion properties, better bond to the weak support point area of ​​the matrix silicon carbide coating, and improve the thermal shock resistance and anti-oxidation performance of the silicon carbide product.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a hot melt adhesive composition, which comprises, by weight, 60-90 parts of a base resin, 12-20 parts of a tackifier, 0.1-0.5 parts of a plasticizer, and 0.1-2 parts of an antioxidant; the base resin is a polymer resin with a molecular weight of 50,000-100,000 g / mol; the plasticizer comprises a petroleum-based plasticizer and an ester plasticizer.

[0007] The present invention also provides a hot melt adhesive, which is prepared using the hot melt adhesive composition described in the first aspect of the present invention.

[0008] The second aspect of the present invention provides the hot melt adhesive composition described in the first aspect, or the use of the hot melt adhesive prepared from the hot melt adhesive composition in a method for sandblasting the surface of a silicon carbide coating.

[0009] A third aspect of the present invention provides a method for sandblasting a silicon carbide coating surface, comprising the following steps:

[0010] (1) preparing hot melt adhesive;

[0011] (2) Preparing a stopper: testing a first aperture of a support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point;

[0012] (3) Hot melt adhesive coating: placing the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; heating the hot melt adhesive of step (1) to the first temperature to melt and then injecting it into the second aperture of the stopper to cover the supporting point

[0013] (4) Sandblasting: After the hot melt adhesive is cured, remove the limiter and sandblast the surface of the silicon carbide coating;

[0014] (5) Removing hot melt adhesive: After the silicon carbide coating is sandblasted, it is heated to a second temperature to melt the hot melt adhesive and separate it from the supporting point.

[0015] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0016] (1) The hot melt adhesive composition provided by the present invention comprises a base resin and auxiliary agents such as a tackifier, a plasticizer and an antioxidant, so that the hot melt adhesive has better adhesive properties.

[0017] (2) The method for sandblasting the surface of the silicon carbide coating provided by the present invention uses hot melt adhesive to be coated on the supporting points of the substrate to protect the weak areas of the supporting points of the silicon carbide coating of the substrate.

[0018] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION

[0019] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0020] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0021] The first aspect of the present invention provides a hot melt adhesive composition, which comprises, by weight, 60-90 parts (e.g., 60 parts, 65 parts, 70 parts, 75 parts, 80 parts) of a base resin, 12-20 parts (e.g., 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts) of a tackifier, 0.1-0.5 parts (0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts) of a plasticizer, and 0.1-2 parts (0.1 parts, 0.3 parts, 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts) of an antioxidant; the base resin is a polymer resin with a molecular weight of 50,000-100,000 g / mol; the plasticizer comprises a petroleum-based plasticizer and an ester plasticizer.

[0022] In the present invention, the high molecular weight matrix resin will give the hot melt adhesive better mechanical strength, durability and bonding performance. The hot melt adhesive is used in the sandblasting process of the silicon carbide coating to prevent the hot melt adhesive from falling off, better protect the supporting points of the matrix, and improve the thermal shock resistance and oxidation resistance of the silicon carbide product. However, the medium and low molecular weight matrix resin hot melt adhesive may result in poor bonding strength, and it is easy to fall off from the group due to the sandblasting pressure during the sandblasting process, and it cannot protect the supporting points of the matrix well.

[0023] In the present invention, the petroleum-based plasticizer and the ester plasticizer are used in combination in the hot melt adhesive. The petroleum-based plasticizer can lower the melting point of the hot melt adhesive, allowing the hot melt adhesive to melt quickly and be convenient to use, and can also improve the flexibility and impact resistance of the hot melt adhesive; the ester plasticizer can improve the adhesion and durability of the hot melt adhesive. Therefore, the use of the petroleum-based plasticizer and the ester plasticizer in combination can improve the impact resistance of the hot melt adhesive, improve the adhesion between the hot melt adhesive and the support point of the substrate, thereby preventing the hot melt adhesive from falling off, better protecting the support point of the substrate, and improving the thermal shock resistance and anti-oxidation performance of the silicon carbide product.

[0024] The present invention also provides a hot melt adhesive, which is prepared by using the hot melt adhesive composition described in the first aspect of the present invention. In the present invention, "hot melt adhesive composition" may refer to "hot melt adhesive", and the specific meaning is determined according to the context.

[0025] The hot melt adhesive prepared from the hot melt adhesive composition is a plastic adhesive whose physical state changes with temperature within a certain temperature range, while its chemical properties remain unchanged. Hot melt adhesives can be divided into several categories according to the base resin, such as ethylene vinyl acetate (EVA), polyester (PET), polyamide (PA) and polyurethane (PU).

[0026] Ethylene-vinyl acetate hot melt adhesive has good electrical and bonding properties, but poor heat resistance and elasticity; polyester and polyamide hot melt adhesives have high bonding strength and a wide range of applications, but their melt viscosity is high; polyurethane hot melt adhesive has good toughness, excellent low temperature resistance, easy application, strong bonding force, and a wide range of bonding substrates. It is a hot melt adhesive with excellent comprehensive performance and has been widely studied and applied. After the hot melt adhesive is heated to a certain temperature, it can melt into a viscous liquid. After wetting the adherend, it can be cooled to room temperature to achieve bonding to the adherend. It is usually solid at room temperature (solid content 100%).

[0027] In some embodiments, the hot melt adhesive composition includes 75-85 parts of base resin, 14-16 parts of tackifier, 0.2-0.4 parts of plasticizer, and 0.8-1.2 parts of antioxidant by weight. The ratio of base resin, tackifier, plasticizer, and antioxidant in the hot melt adhesive composition is further preferred to further improve the adhesive properties of the hot melt adhesive.

[0028] In some embodiments, the base resin is selected from at least one of polyolefins and copolymers thereof, thermoplastic elastomers, cellulose derivatives, polyamide resins, polyester resins, and polyurethane resins.

[0029] Exemplarily, the polyolefin and copolymers thereof include ethylene-vinyl acetate copolymer resin (EVA), low molecular weight polyethylene (PE), ethylene-ethyl acrylate copolymer resin (EEA), random polypropylene (APP), ethylene-acrylic acid copolymer (EAA), and the like.

[0030] Exemplarily, the thermoplastic elastomer includes butyl rubber (BR), styrene-butadiene block copolymer (SBS), styrene-isoprene block copolymer (SIS), and the like.

[0031] Matrix resin plays a key role in hot melt adhesive. Matrix resin can provide bonding strength and viscosity for hot melt adhesive, making it easier to apply hot melt adhesive on the supporting points of the substrate. After the hot melt adhesive is cured, the bonding force between the hot melt adhesive and the supporting points is stronger and not easy to fall off, thereby better protecting the weak areas of the substrate coating.

[0032] In some embodiments, the tackifier is selected from at least one of paraffin wax, terpene resin and modified terpene resin, petroleum resin, rosin and modified rosin, rosin resin, thermoplastic phenolic resin and polyisobutylene. The tackifier plays a role in adjusting viscosity, enhancing bonding strength, improving adhesion, etc. in the hot melt adhesive. The tackifier works together with the base resin to make the hot melt adhesive have better bonding properties, and further better protect the weak areas of the base coating.

[0033] In some embodiments, the petroleum-based plasticizer is selected from at least one of paraffin wax, microcrystalline wax, and polyethylene wax.

[0034] In some embodiments, the plasticizer is selected from at least one of dibutyl phthalate, dioctyl phthalate, and butyl benzyl phthalate.

[0035] Plasticizers play a role in hot melt adhesives in improving flexibility, plasticity, adjusting viscosity, increasing bonding strength and adjusting curing time. Plasticizers work together with base resins and tackifiers to give hot melt adhesives good bonding properties and suitable curing time, thereby comprehensively improving the effect of hot melt adhesives in protecting base support points.

[0036] In some embodiments, the mass ratio of the petroleum-based plasticizer to the ester plasticizer is 1:(0.8-1.2). When the mass ratio of the two plasticizers is within the above range, the impact resistance of the hot melt adhesive can be further improved, and the adhesion between the hot melt adhesive and the substrate support point can be improved.

[0037] In some embodiments, the antioxidant is selected from at least one of aromatic amines and hindered phenols. Antioxidants play a role in extending the service life, protecting performance stability, improving heat resistance and enhancing weather resistance in hot melt adhesives. Antioxidants can protect hot melt adhesives from oxidation, maintain their performance and improve their application characteristics under various environmental conditions.

[0038] In some embodiments, the aromatic amine antioxidants include N-phenyl-β-naphthylamine, diphenylamine, p-phenylenediamine, dihydroquinoline, 4,4'-bis(ɑ,ɑ-dimethylbenzyl)diphenylamine, tert-butylhydroxyquinolinone, and the like.

[0039] In some embodiments, the hindered phenol antioxidant includes 2,6-di-tert-butyl-p-cresol, o-tert-butylphenol, 3,5-di-tert-butyl-4-hydroxyphenylhydrocinnamic acid C7-C9 branched alkyl ester, 4,4'-methylenebis(2,6-di-tert-butylphenol), and the like.

[0040] Among the types of base resins, tackifiers and plasticizers listed above, after a large number of experimental studies, it was unexpectedly found that when the base resin is EVA, the tackifier is terpene resin, the plasticizer is paraffin and dibutyl phthalate, and the antioxidant is N-phenyl-β-naphthylamine, the hot melt adhesive has the best bonding performance. The hot melt adhesive can better bond to the weak areas of the supporting points of the base silicon carbide coating, and better improve the thermal shock resistance and antioxidant properties of the silicon carbide product.

[0041] In some embodiments, the hot melt adhesive comprises 75-85 parts of EVA, 13-16 parts of terpene resin, 0.2-0.4 parts of dibutyl phthalate, and 0.8-1.2 parts of N-phenyl-β-naphthylamine by weight. The ratio of the base resin, tackifier, plasticizer, and antioxidant in the hot melt adhesive is further optimized to further improve the adhesive properties of the hot melt adhesive.

[0042] In some embodiments, the plasticizer accounts for 0.2% to 0.6% of the mass of the matrix resin. When the mass ratio of the matrix resin to the tackifier is within the above range, the bonding force between the hot melt adhesive and the matrix support point after curing can be controlled to prevent the hot melt adhesive from falling off.

[0043] The second aspect of the present invention provides the use of the hot melt adhesive described in the first aspect in a method for sandblasting the surface of a silicon carbide coating.

[0044] In the prior art, some means of protecting support points take a long time and are complicated to operate, and the improvement effect is not good. The present invention has found that hot melt adhesive is used to protect the support points of the substrate. The curing time of hot melt adhesive is short, which saves processing time and the operation method is relatively simple. Hot melt adhesive is used in the sandblasting method of the silicon carbide coating surface to better protect the weak areas of the substrate coating.

[0045] A third aspect of the present invention provides a method for sandblasting a silicon carbide coating surface, comprising the following steps:

[0046] (1) preparing hot melt adhesive;

[0047] (2) Preparing a stopper: testing a first aperture of a support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point;

[0048] (3) Hot melt adhesive coating: placing the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; heating the hot melt adhesive of step (1) to the first temperature and then melting it to inject it into the second aperture of the stopper to cover the supporting point;

[0049] (4) Sandblasting: After the hot melt adhesive is cured, remove the stopper and sandblast the surface of the silicon carbide coating;

[0050] (5) Removing hot melt adhesive: After the silicon carbide coating is sandblasted, it is heated to a second temperature to melt the hot melt adhesive and separate it from the supporting point.

[0051] In some embodiments, in step (1), according to the formula of the hot melt adhesive, 60-90 parts of base resin, 12-20 parts of tackifier, 0.1-0.5 parts of plasticizer, and 0.1-2 parts of antioxidant are weighed to prepare the hot melt adhesive for use.

[0052] In some embodiments, in step (2), before sandblasting, the hot melt adhesive is first accurately coated on the support points of the substrate using a limiting member. This can prevent the hot melt adhesive from flowing and being unable to effectively cover the support points of the substrate, or prevent the parts of the support points that do not need to be shielded and protected from being covered by the hot melt adhesive, thereby improving the efficiency of subsequent sandblasting.

[0053] In some embodiments, in step (2), the size of the second aperture of the limiting member is limited to be no less than the size of the first aperture of the supporting point, so that the hot melt adhesive can completely cover the supporting point of the substrate, thereby better protecting the supporting point from being damaged by the high-speed impact of sandblasting and exposing the graphite substrate.

[0054] In some embodiments, in step (2), the thickness of the stopper is between 0.5-5 mm. The stopper can be made of epoxy resin or other materials. When the thickness of the stopper is within the above range, it can ensure that the thickness of the hot melt adhesive covering the support point of the substrate is appropriate, avoiding damage caused by high-speed impact of sandblasting due to too small thickness, and avoiding waste of hot melt adhesive and prolonged curing time due to too large thickness, which affects processing efficiency.

[0055] In some embodiments, in step (2), the size of the second aperture is 1-5 mm larger than the size of the first aperture, so that the hot melt adhesive can completely cover the substrate support points, better protecting the support points from being damaged by the high-speed impact of sandblasting and exposing the graphite substrate.

[0056] In some embodiments, in step (3), the first temperature is 50-100° C., which is the temperature at which the hot melt adhesive melts. The first temperature may vary depending on the hot melt adhesive matrix resin or the formulation ratio. The melting temperature of the hot melt adhesive is relatively low, which facilitates application to the support points of the substrate.

[0057] In some embodiments, in step (3), the coating method is spot coating and / or spray coating. For the purpose of more precise coating, spot coating is more preferred, for example, using a tool to coat the melted hot melt adhesive on the supporting points.

[0058] In some embodiments, in step (4), the thickness of the hot melt adhesive after curing is 20 μm-100 μm, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm. When the thickness of the hot melt adhesive after curing is controlled within the above range, it can be avoided that the thickness is too thin to affect the protective effect of the substrate during sandblasting.

[0059] In some embodiments, in step (4), the process parameters of sandblasting are not limited and can be freely selected according to needs. For example, the process parameters of sandblasting may include: sandblasting pressure of 0.5-5.5 kg / cm 2 , the sandblasting mesh number is 80-300 mesh.

[0060] In some embodiments, the sandblasting material is selected from at least one of silica sand, glass beads, steel sand and corundum. In the present invention, since the silicon carbide coating is subjected to sandblasting, silica sand, such as silicon carbide fine sand, is preferred.

[0061] In some embodiments, in step (5), the second temperature is 50-100°C, and the holding time is 3-30 minutes. The second temperature is the temperature at which the cured hot melt adhesive melts again, which is substantially the same as the first temperature, or the second temperature is greater than the first temperature, and the holding time is greater than 3 minutes to ensure that the hot melt adhesive is completely melted, so as to separate the hot melt adhesive from the supporting point.

[0062] In some embodiments, in step (5), the method of separating the hot melt adhesive from the supporting point includes suction and / or scraping. For example, the melted hot melt adhesive is sucked out by a tool and then removed.

[0063] In some embodiments, step (5) further comprises the step of removing residual glue by ultrasonic cleaning: the cleaning temperature is 50-100°C, and the ultrasonic time is 3-30 minutes. In order to avoid some residual glue remaining on the surface of the silicon carbide product, the product can also be treated to remove the residual glue, such as water bath ultrasonic cleaning. When the water bath cleaning temperature and ultrasonic time are kept within the above range, the residual glue on the surface of the product can be better removed.

[0064] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0065] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0066] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0067] Example 1

[0068] (1) Hot melt adhesive: 80 parts by weight of EVA (molecular weight 80,000), 15 parts by weight of tackifier terpene resin, 0.15 parts by weight of plasticizer paraffin and 0.15 parts by weight of dibutyl phthalate, and 1 part by weight of antioxidant N-phenyl-β-naphthylamine;

[0069] (2) Preparing a stopper: testing the first aperture of the support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point; the stopper is made of epoxy resin; and the thickness of the stopper is 3 mm;

[0070] (3) Spot coating: Place the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; Place a small amount of solid hot melt adhesive in a beaker, then transfer to a constant temperature water bath, heat to 50-100°C to melt the hot melt adhesive, then use a syringe to draw a small amount of hot melt adhesive and inject it into the second aperture of the stopper to cover the supporting point. After the hot melt adhesive cools and hardens, remove the stopper for subsequent sandblasting;

[0071] (4) Sand blasting: Open the air valve and make the air inlet pressure gauge point to 8kg / cm 2 , turn on the power switch of the sandblasting machine, adjust the pressure regulating valve so that the pointer of the sandblasting pressure gauge points to 3kg / cm 2 ; The mesh number of silicon carbide used is about 200 meshes, and the inner and outer glass windows are wiped with a dust-free cloth; open the hatch and put in the product, close the hatch, and lock the lock; put both hands into the sandblasting machine gloves, hold the product in the left hand, hold the sandblasting machine nozzle in the right hand, and step on the sandblasting pedal with the right foot to sandblast the product;

[0072] (5) Glue removal: After sandblasting, place the product in a blast oven and heat it to 80°C for about 20 minutes, then take out the hot melt adhesive and use a needle to absorb it; then place the product in an ultrasonic cleaner to clean the remaining hot melt adhesive, the water temperature is 80°C, ultrasonic for about 20 minutes, and then take out the sample.

[0073] Example 2

[0074] (1) Hot melt adhesive: 60 parts by weight of PE (molecular weight 60,000), 20 parts by weight of tackifier thermoplastic phenolic resin, 0.05 parts by weight of plasticizer microcrystalline wax and 0.05 parts by weight of dioctyl phthalate, and 2 parts by weight of antioxidant 2,6-di-tert-methyl phenol;

[0075] (2) Preparing a stopper: testing the first aperture of the support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point; the stopper is made of epoxy resin; and the thickness of the stopper is 0.5 mm;

[0076] (3) Spot coating: Place the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; Place a small amount of solid hot melt adhesive in a beaker, then transfer to a constant temperature water bath, heat to 50-100°C to melt the hot melt adhesive, then use a syringe to draw a small amount of hot melt adhesive and inject it into the second aperture of the stopper to cover the supporting point. After the hot melt adhesive cools and hardens, remove the stopper for subsequent sandblasting;

[0077] (4) Sand blasting: Open the air valve and make the air inlet pressure gauge point to 5kg / cm 2 , turn on the power switch of the sandblasting machine, adjust the pressure regulating valve so that the pointer of the sandblasting pressure gauge points to 0.5kg / cm 2 ; The mesh number of silicon carbide used is about 300 meshes, and the inner and outer glass windows are wiped with a dust-free cloth; open the hatch and put in the product, close the hatch, and lock the lock; put both hands into the sandblasting machine gloves, hold the product in the left hand, hold the sandblasting machine nozzle in the right hand, and step on the sandblasting pedal with the right foot to sandblast the product;

[0078] (5) Glue removal: After sandblasting, place the product in a blast oven and heat it to 100°C for about 10 minutes, then take out the hot melt adhesive and absorb it with a needle; then place the product in an ultrasonic cleaner to clean the remaining hot melt adhesive, the water temperature is 60°C, and the ultrasonic cleaning is performed for about 30 minutes, and then the sample is taken out.

[0079] Example 3

[0080] (1) Hot melt adhesive: 90 parts by weight of styrene-butadiene block copolymer (SBS) (molecular weight 90,000), 12 parts by weight of tackifier petroleum resin, 0.25 parts by weight of plasticizer polyethylene wax and 0.25 parts by weight of butyl benzyl phthalate, and 0.1 parts by weight of antioxidant 4,4'-bis(ɑ,ɑ-dimethylbenzyl) diphenylamine;

[0081] (2) Preparing a stopper: testing the first aperture of the support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point; the stopper is made of epoxy resin; and the thickness of the stopper is 5 mm;

[0082] (3) Spot coating: Place the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; Place a small amount of solid hot melt adhesive in a beaker, then transfer to a constant temperature water bath, heat to 50-100°C to melt the hot melt adhesive, then use a syringe to draw a small amount of hot melt adhesive and inject it into the second aperture of the stopper to cover the supporting point, wait for the hot melt adhesive to cool and harden, then perform sandblasting, remove the stopper, and perform subsequent sandblasting;

[0083] (4) Sand blasting: Open the air valve and make the air inlet pressure gauge point to 10kg / cm 2 , turn on the power switch of the sandblasting machine, adjust the pressure regulating valve so that the pointer of the sandblasting pressure gauge points to 5.5kg / cm 2 ; The mesh number of silicon carbide used is about 100 meshes, and the inner and outer glass windows are wiped with a dust-free cloth; open the hatch and put in the product, close the hatch, and lock the lock; put both hands into the sandblasting machine gloves, hold the product in the left hand, hold the sandblasting machine nozzle in the right hand, and step on the sandblasting pedal with the right foot to sandblast the product;

[0084] (5) Glue removal: After sandblasting, place the product in a blast oven and heat it to 70°C for about 20 minutes, then take out the hot melt adhesive and use a syringe to absorb it; then place the product in an ultrasonic cleaner to clean the remaining hot melt adhesive, the water temperature is 50°C, and the ultrasonic cleaner is used for about 30 minutes, and then the sample is taken out.

[0085] Example 4 Group

[0086] The method is carried out with reference to Example 1, except that the type or content of the base resin is different, as follows:

[0087] Example 4a: EVA is replaced by an equal amount of EEA;

[0088] Example 4b: EVA is replaced by an equal amount of PE;

[0089] Example 4c: EVA is 60 parts by weight;

[0090] Example 4d: EVA is 90 parts by weight.

[0091] Example 5 Group

[0092] The method is carried out with reference to Example 1, except that the type or content of the tackifier is different, as follows:

[0093] Example 5a: An equal amount of thermoplastic phenolic resin replaces the terpene resin;

[0094] Example 5b: An equal amount of petroleum resin replaces the terpene resin;

[0095] Example 5c: 13 parts by weight of terpene resin;

[0096] Example 5d: The terpene resin is 18 parts by weight.

[0097] Example 6 Group

[0098] The same method is carried out with reference to Example 1, except that the type or content of the plasticizer is different, as follows:

[0099] Embodiment 6a: The plasticizer is 0.05 weight part of paraffin wax and 0.25 weight part of dibutyl phthalate;

[0100] Example 6b: The plasticizer is 0.25 parts by weight of paraffin and 0.05 parts by weight of dibutyl phthalate.

[0101] Example 7 Group

[0102] The method is carried out with reference to Example 1, except that the type or content of the antioxidant is different, as follows:

[0103] Example 7a: An equal amount of p-phenylenediamine replaces N-phenyl-β-naphthylamine;

[0104] Example 7b: An equal amount of 2,6-di-tert-p-cresol is substituted for N-phenyl-β-naphthylamine;

[0105] Example 7c: N-phenyl-β-naphthylamine is 0.5 parts by weight;

[0106] Example 7d: N-phenyl-β-naphthylamine is 1.5 parts by weight.

[0107] Example 8 Group

[0108] The method is carried out with reference to Example 1, except that the molecular weight of the base resin is different, as follows:

[0109] Example 8a: The molecular weight of EVA is 50,000;

[0110] Example 8b: The molecular weight of EVA is 100,000 g / mol.

[0111] Comparative Example 1

[0112] Do not apply hot melt adhesive to the supporting points, but sandblast directly.

[0113] Comparative Example 2

[0114] The method is carried out with reference to Example 1, except that the hot melt adhesive formula is: 50 parts by weight of EVA, 30 parts by weight of tackifier terpene resin, 0.3 parts by weight of plasticizer dibutyl phthalate, and 1 part by weight of antioxidant N-phenyl-β-naphthylamine.

[0115] Comparative Example 3

[0116] The same method is carried out as in Example 1, except that an equal amount of epoxy resin replaces the hot melt adhesive.

[0117] Comparative Example 4

[0118] The same procedure was followed as in Example 1, except that the type of plasticizer was changed.

[0119] Comparative Example 4a: The plasticizer is 0.3 parts by weight of paraffin;

[0120] Comparative Example 4b: The plasticizer is 0.3 parts by weight of dibutyl phthalate.

[0121] Comparative Example 5

[0122] The method is carried out with reference to Example 1, except that the molecular weight of the base resin is different, as follows:

[0123] Comparative Example 5a: The molecular weight of EVA is 1000;

[0124] Comparative Example 5b: The molecular weight of EVA is 2,000 g / mol.

[0125] Comparative Example 6

[0126] The process is carried out in accordance with Example 1, except that no limiting member is used in step (2).

[0127] The performance of the silicon carbide products obtained in the above embodiments and comparative examples was tested using the following test methods:

[0128] (1) Thermal shock performance test

[0129] The silicon carbide product was kept at 400°C for 15 minutes and then air-cooled. The test was repeated for multiple cycles until cracks appeared on the surface of the silicon carbide product. The number of cycles was recorded as the number of thermal shock failures. The thermal shock performance of the product was evaluated by the number of thermal shock failures. The greater the number of thermal shock failures, the better the thermal shock performance. The test results are recorded in Table 1.

[0130] (2) Antioxidant performance test

[0131] The silicon carbide product was continuously ablated at 800°C for 24 hours, and then weighed after cooling. The weight loss of the sample was recorded to evaluate the antioxidant performance of the product. Oxidation weight loss rate = (product weight before ablation - product weight after ablation) / product weight before ablation *‰. The smaller the weight loss rate of the sample, the better the antioxidant performance. The test results are recorded in Table 1.

[0132] Table 1

[0133]

[0134]

[0135] As can be seen from Table 1, the thermal shock and anti-oxidation properties in Comparative Example 1 are the worst, indicating that using hot melt adhesive or epoxy resin adhesive to protect the product support points during sandblasting will improve the thermal shock and anti-oxidation properties; the thermal shock and anti-oxidation properties of the product in Example 1 are better than those in Comparative Example 3, indicating that the protection effect of using hot melt adhesive on the support points is better than that of epoxy resin adhesive. After comparing the EVA, EEA, and PE matrix resins in Example 1, Example 4a, and Example 4b, it is found that the EVA matrix resin has the best protection effect on the support points and the best thermal shock and anti-oxidation properties. In Example 1, Example 4c, and Example 4d, the effects of different EVA matrix resin contents on the support points were compared, and it was found that when the EVA content was 80 weight%, the product had the best thermal shock and anti-oxidation properties.

[0136] In Example 1, Example 5a, Example 5b, Example 5c, and Example 5d, the effects of the type or content of the tackifier on the support point were compared, and it was found that when the tackifier terpene resin was 15 parts by weight, the thermal shock and antioxidant properties of the product were the best. In Example 1, Example 6a, and Example 6b, the effects of the type or content of the plasticizer on the support point were compared, and it was found that when the paraffin wax was 0.15 parts by weight and the dibutyl phthalate was 0.15 parts by weight, the thermal shock and antioxidant properties of the product were the best. In Example 1, Example 7a, Example 7b, Example 7c, and Example 7d, the effects of the type or content of the antioxidant on the support point were compared, and it was found that when the N-phenyl-β-naphthylamine was 1 part by weight, the thermal shock and antioxidant properties of the product were the best. In Example 1, Comparative Example 5a, Comparative Example 5b, Example 8a, and Example 8b, the effects of the molecular weight of EVA on the support point were compared, and it was found that the thermal shock and antioxidant properties of the product after sandblasting with high molecular weight EVA were better. In Example 1 and Comparative Example 6, the effects of using or not using a stopper on the supporting point were compared, and it was found that after using the stopper, the thermal shock and oxidation resistance of the product were better.

[0137] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A hot melt adhesive composition, characterized in that: By weight, it includes 60-90 parts of base resin, 12-20 parts of tackifier, 0.1-0.5 parts of plasticizer, and 0.1-2 parts of antioxidant; The base resin is a polymer resin with a molecular weight of 50,000-100,000 g / mol; The plasticizers include petroleum-based plasticizers and ester plasticizers.

2. The hot melt adhesive composition according to claim 1, characterized in that: The base resin is selected from at least one of polyolefins and copolymers thereof, thermoplastic elastomers, cellulose derivatives, polyamide resins, polyester resins and polyurethane resins; and / or, the tackifier is selected from at least one of paraffin wax, terpene resin and modified terpene resin, petroleum resin, rosin and modified rosin, rosin resin, thermoplastic phenolic resin and polyisobutylene; And / or, the petroleum-based plasticizer is selected from at least one of paraffin wax, microcrystalline wax, and polyethylene wax; And / or, the ester plasticizer is at least one selected from dibutyl phthalate, dioctyl phthalate and butyl benzyl phthalate; And / or, the antioxidant is selected from at least one of aromatic amines and hindered phenols.

3. The hot melt adhesive composition according to claim 1, characterized in that: The plasticizer accounts for 0.2% to 0.6% of the mass of the base resin; and / or, the mass ratio of petroleum-based plasticizer to ester plasticizer is 1:(0.8-1.2); And / or, the hot melt adhesive composition comprises EVA, terpene resin, paraffin, dibutyl phthalate, and N-phenyl-β-naphthylamine in parts by weight.

4. Use of the hot melt adhesive composition according to any one of claims 1 to 3 in a method for sandblasting the surface of a silicon carbide coating.

5. A method for sandblasting a silicon carbide coating surface, characterized in that: The following steps are involved: (1) preparing hot melt adhesive; (2) Preparing a stopper: testing a first aperture of a support point on the surface of the silicon carbide coating, and drilling a hole in the stopper according to the size of the first aperture; wherein the size of the second aperture of the stopper is not less than the size of the first aperture of the support point; (3) Hot melt adhesive coating: placing the stopper of step (2) at the supporting point on the surface of the silicon carbide coating, with the axis of the second aperture coinciding with the axis of the first aperture; heating the hot melt adhesive of step (1) to the first temperature and then melting it to inject it into the second aperture of the stopper to cover the supporting point; (4) Sandblasting: After the hot melt adhesive is cured, remove the limiter and sandblast the surface of the silicon carbide coating; (5) Removing hot melt adhesive: After the silicon carbide coating is sandblasted, it is heated to a second temperature to melt the hot melt adhesive and separate it from the supporting point.

6. The method according to claim 5, characterized in that In step (2), the thickness of the stopper is between 0.5 and 5 mm; And / or, in step (2), the size of the second aperture is 1-5 mm larger than the size of the first aperture.

7. The method according to claim 5, characterized in that In the step (3), the first temperature is 50-100° C.; And / or, the hot melt adhesive coating method is spot coating and / or spray coating; And / or, in step (3), the thickness of the hot melt adhesive after curing is 20 μm-100 μm.

8. The method according to any one of claims 5 to 7, characterized in that: In step (4), the process parameters of sandblasting include: sandblasting pressure of 0.5-5.5kg / cm 2 , the sandblasting mesh number is 80-300 mesh; And / or, the material for sandblasting is selected from at least one of silica sand, glass beads, steel sand and corundum.

9. The method according to any one of claims 5 to 7, characterized in that: In the step (5), the second temperature is 50-100° C., and the insulation time is 3 min-30 min; And / or, the method of separation includes suction and / or scraping.

10. The method according to any one of claims 5 to 7, characterized in that: The step (5) further comprises the step of removing residual glue by ultrasonic cleaning: the cleaning temperature is 50-100° C., and the ultrasonic time is 3-30 min.