PAA binder and preparation method thereof, binder composition, negative pole piece and battery
By using PAA binder obtained by copolymerizing unsaturated acid with ethylene oxide or acrylonitrile in sodium ion batteries, the problem of poor processing performance after the surface density of sodium ion batteries is increased, and the ion conductivity of the negative electrode sheet is improved and cycling performance, achieving better electrochemical performance.
Patent Information
- Application Number
- CN202411386416.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
After the surface density of sodium ion batteries increases, processing problems are prone to occur, such as low peeling force, coating cracking, diaphragm resistance, etc., and their performance shows that the circulation capacity retention rate is fast attenuated, and processing flexibility and kinetic performance need to be improved.
Using PAA binder obtained by copolymerizing unsaturated acid or unsaturated acid salt with ethylene oxide or acrylonitrile, the processing performance of the electrode sheet is improved by branched chain copolymerization or alternating arrangement, and PAA bonding is added to the negative electrode sheet. Agent is used to enhance ion conductivity.
It effectively improves the cracking problem under thick surface density, improves the charge transfer impedance of the negative electrode, improves the rate performance and capacity attenuation during the cycle, and improves the electrochemical performance of sodium ion batteries.
Smart Images

Figure CN119081589A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a PAA binder and a preparation method thereof, a binder composition, a negative electrode sheet and a battery. Background Art
[0002] Sodium-ion batteries have similar theoretical foundations to lithium-ion batteries, relatively low budgets, and abundant sodium resources. They are recognized as the most competitive alternative to lithium-ion batteries when lithium ore prices are high. Among the positive electrode materials of sodium-ion batteries, polyanionic sodium iron pyrophosphate materials have the advantages of stable structure, long cycle period, and easy synthesis. They have broad application space in energy storage application scenarios. As the cost requirements of the energy storage market become lower and lower, in addition to reducing costs by the main materials of the positive and negative electrodes and electrolytes, it is becoming more and more urgent to reduce costs by increasing the surface density.
[0003] However, increasing the surface density can easily lead to various processing and performance problems. Among them, processing is prone to problems such as low peeling force, coating cracking, and high film resistance. Performance is prone to abnormalities such as rapid decay of capacity retention during the cycle. Improving the negative electrode dynamics can improve the reversible capacity decay caused by the charge rate and polarization of the battery cell. Improving the adhesive peeling force can improve the abnormal diving in the late cycle.
[0004] Therefore, there is an urgent need for a sodium battery negative electrode binder and a negative electrode plate to improve the processing flexibility and kinetic performance of the sodium ion battery while ensuring the electrochemical performance of the sodium ion battery. Summary of the invention
[0005] The purpose of the present invention is to provide a PAA binder and a preparation method thereof, a binder composition, a negative electrode plate and a battery, so as to solve the deficiencies in the prior art and effectively improve the processing flexibility and dynamic performance of the sodium ion battery while ensuring the electrochemical performance of the sodium ion battery.
[0006] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a PAA binder obtained by copolymerizing a first monomer and a second monomer, wherein the first monomer and the second monomer constitute a chain segment in the form of branched copolymerization or alternating arrangement; the first monomer is an unsaturated acid or an unsaturated acid salt, and the second monomer is ethylene oxide or acrylonitrile.
[0007] According to a PAA binder provided by the present invention, the molecular weight of the PAA binder is 10,000 to 200,000; and / or the viscosity of the PAA binder is 5,000 to 20,000 mPas.
[0008] According to a PAA binder provided by the present invention, the first monomer includes one or more of acrylic acid, acrylic acid salt, methacrylic acid, methacrylic acid salt, propylene sulfonic acid, propylene sulfonate, methacrylic acid, methacrylic acid, N-vinyl pyrrolidone itaconic acid, itaconic acid salt, maleic acid and maleate; preferably acrylic acid.
[0009] According to a PAA binder provided by the present invention, the molar ratio of the first monomer to the second monomer is (2-8): (2-8).
[0010] According to a PAA binder provided by the present invention, when the molar ratio of the first monomer to the second monomer is (6-8): (2-4), the PAA binder forms a branched copolymer structure; when the molar ratio of the first monomer to the second monomer is (2-4): (6-8), the PAA binder forms an alternating arrangement structure.
[0011] In a second aspect, the present invention provides a method for preparing the PAA binder, comprising: mixing the first monomer, the second monomer, a first solvent and an initiator, and performing a polymerization reaction at 40 to 100 degrees Celsius and 0.1 to 1 MPa; preferably, the first solvent comprises water, and the initiator comprises one or more of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and benzoyl peroxide.
[0012] According to the present invention, a method for preparing a PAA binder comprises: mixing the first monomer, the second monomer, the first solvent, the first dispersant, the leveling wetting agent, the defoaming agent and the initiator, and performing a polymerization reaction at 40-100 degrees Celsius and 0.1-1 MPa; more preferably, the first dispersant comprises water, the leveling wetting agent comprises one or more of sodium dodecyl sulfonate (SDS), sodium dodecylbenzene sulfonate (LAS), sodium secondary alkyl sulfonate (SAS) and sodium α-olefin sulfonate (AOS), and the defoaming agent comprises one or more of polyether silicone, gemini glycol polyether and star polyether.
[0013] In a third aspect, the present invention provides an adhesive composition, comprising the PAA adhesive and a first adhesive; the first adhesive comprises sodium polyacrylate and / or styrene butadiene.
[0014] In a fourth aspect, the present invention provides a negative electrode plate comprising the PAA binder or the binder composition.
[0015] In a fifth aspect, the present invention provides a method for preparing the negative electrode sheet, comprising: mixing a sodium negative electrode active material, the binder composition according to claim 7, a second dispersant, and a second solvent, coating the obtained mixed slurry on a current collector, and then drying to obtain the negative electrode sheet; the binder composition comprises the PAA binder according to any one of claims 1 to 4 and the first binder; preferably, the mass of the PAA binder is 0.2wt% to 0.6wt% of the total solid phase mass of the mixed slurry.
[0016] In a sixth aspect, the present invention provides a battery comprising the negative electrode plate.
[0017] The PAA binder and preparation method thereof, binder composition, negative electrode plate and battery provided by the present invention synthesize EO segments or cyano high polar groups at the molecular level, and the obtained PAA binder contains a structure of soft and hard alternating arrangement, has good processing performance, can improve the cracking problem under thick surface density, and has excellent repeatability. At the same time, because EO segments or acrylonitrile segments are alternately grafted on its main chain, it has good ion conductivity, can improve the negative electrode charge transfer impedance, and further improve the rate performance and capacity attenuation caused by polarization during the cycle process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 It is a schematic diagram of the copolymerization of EO chains and PAA chains in the PAA binder provided by the present invention.
[0020] Figure 2 It is a schematic diagram showing that EO chains and PAA in the PAA binder provided by the present invention are alternately arranged on the main chain. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] In order to improve the processing problem of sodium ion batteries in the prior art, PAA binders are tried. For example, patent application CN202410411355.3 discloses a sodium negative electrode binder, a sodium negative electrode sheet, and a sodium ion battery, wherein the sodium negative electrode binder includes a first binder and carboxylated styrene-butadiene rubber, and the first binder includes a mixture and / or a composite of chitosan and aqueous sodium polyacrylate. That is, the sodium negative electrode binder in CN202410411355.3 is a mixture of chitosan, aqueous sodium polyacrylate, and carboxylated styrene-butadiene rubber by physical stirring; the present invention finds that the prior art such as CN202410411355.3 uses physical mixing of conventional binders rather than synthesis at the molecular level, so problems such as uneven distribution of various parts are prone to occur, thereby affecting processing performance and electrochemical performance.
[0023] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a PAA binder obtained by copolymerizing a first monomer and a second monomer, wherein the first monomer and the second monomer constitute a chain segment in the form of branched copolymerization or alternating arrangement; the first monomer is an unsaturated acid or an unsaturated acid salt, and the second monomer is ethylene oxide or acrylonitrile.
[0024] The present invention finds that by alternately grafting EO segments or acrylonitrile segments on the main chain of the first monomer, the processing performance of the electrode can be greatly improved and the cracking problem under thick surface density can be improved; at the same time, since EO segments or acrylonitrile segments are alternately grafted on its main chain, it has good ion conductivity, which can improve the negative electrode charge transfer impedance, thereby improving the rate performance and the capacity attenuation caused by polarization during the cycle process.
[0025] In the present invention, the branched copolymerization method specifically refers to: the main chain of the copolymer is composed of the first monomer, and there is a short branch formed by an ethylene oxide monomer or an acrylonitrile monomer for every first monomer unit, the length of the branch is 1 to 4 second monomer units, and the branches are evenly distributed on the main chain. The alternating arrangement method specifically refers to: the second monomer and the first monomer are alternately distributed.
[0026] According to a preferred embodiment provided by the present invention, the segments of the PAA binder are arranged alternately.
[0027] The present invention finds that the alternating arrangement method can further improve the processing performance and improve the cracking problem under thick surface density because it contains a soft and hard alternating arrangement structure.
[0028] It has a structure with alternating soft and hard arrangements.
[0029] According to a preferred embodiment provided by the present invention, the molecular weight of the PAA binder is 10,000 to 200,000; and / or the viscosity of the PAA binder is 5,000 to 20,000 mPas.
[0030] According to a preferred embodiment provided by the present invention, the first monomer includes one or more of acrylic acid, acrylic acid salt, methacrylic acid, methacrylic acid salt, propylene sulfonic acid, propylene sulfonate, methacrylic acid, methacrylic acid, N-vinyl pyrrolidone itaconic acid, itaconic acid salt, maleic acid and maleate; more preferably acrylic acid.
[0031] According to a preferred embodiment provided by the present invention, the molar ratio of the first monomer to the second monomer is (2-8): (2-8).
[0032] According to a preferred embodiment provided by the present invention, when the molar ratio of the first monomer to the second monomer is (6-8): (2-4), the PAA binder forms a branched copolymer structure; when the molar ratio of the first monomer to the second monomer is (2-4): (6-8), the PAA binder forms an alternating arrangement structure.
[0033] In a second aspect, the present invention provides a method for preparing the PAA binder, comprising: mixing the first monomer, the second monomer, a first solvent and an initiator, and performing a polymerization reaction at 40 to 100 degrees Celsius and 0.1 to 1 MPa; preferably, the first solvent comprises water, and the initiator comprises one or more of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and benzoyl peroxide.
[0034] According to a preferred embodiment provided by the present invention, the preparation method of the PAA binder includes: mixing the first monomer, the second monomer, the first solvent, the first dispersant, the leveling wetting agent, the defoaming agent and the initiator, and performing a polymerization reaction at 40-100 degrees Celsius and 0.1-1 MPa; more preferably, the first dispersant includes water, the leveling wetting agent includes one or more of sodium dodecyl sulfonate (SDS), sodium dodecylbenzene sulfonate (LAS), sodium secondary alkyl sulfonate (SAS) and sodium α-olefin sulfonate (AOS), and the defoaming agent includes one or more of polyether silicone, gemini glycol polyether and star polyether.
[0035] In a third aspect, the present invention provides an adhesive composition, comprising the PAA adhesive and a first adhesive; the first adhesive comprises sodium polyacrylate and / or styrene butadiene.
[0036] According to a preferred embodiment of the present invention, in the binder composition, the amount of the PAA binder is 5wt% to 15wt%, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%.
[0037] According to a preferred embodiment provided by the present invention, the first binder is a mixture of sodium polyacrylate and / or styrene butadiene; further preferably, the binder composition comprises the following components in parts by weight: 1.5-1.7 parts of the PAA binder; 1.0-1.4 parts of sodium polyacrylate; Styrene butadiene 0.2~0.4 parts.
[0038] In a fourth aspect, the present invention provides a negative electrode plate comprising the PAA binder or the binder composition.
[0039] In a fifth aspect, the present invention provides a method for preparing the negative electrode sheet, which comprises: mixing a sodium negative electrode active material, the binder composition according to claim 7, a second dispersant and a second solvent, coating the obtained mixed slurry on a current collector, and then drying to obtain the negative electrode sheet; the binder composition comprises the PAA binder according to any one of claims 1 to 4 and the first binder.
[0040] The present invention finds that in the mixed slurry, if the amount of the PAA binder is too low, it cannot significantly improve the ion conductivity, while if the amount is too high, it will occupy more main materials and conductive agents, resulting in poor conductivity. There is an optimal amount range for improving DCR.
[0041] According to a preferred embodiment of the present invention, the mass of the PAA binder is 0.2wt%~0.6wt% of the total mass of the solid phase of the mixed slurry, and more preferably, for example, 0.2wt%~0.4wt%, which can be 0.2wt%, 0.3wt% or 0.4wt%.
[0042] Preferably, the sodium negative electrode active material comprises hard carbon, the second dispersant comprises sodium carboxymethyl cellulose (CMC), and the second solvent comprises water.
[0043] In the present invention, the hard carbon can be prepared by a resin-based synthesis method, a biomass synthesis method or a coal-based synthesis method, which is not limited in the present invention.
[0044] In the present invention, the CMC is selected from one or more of different degrees of substitution, ranging from 0.65 to 0.95. The higher the degree of substitution, the higher the affinity with water.
[0045] Preferably, the amount of CMC is 0.5wt% to 2wt% of the total mass of the solid phase of the mixed slurry, for example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%.
[0046] In the present invention, those skilled in the art can use conventional copolymerization methods disclosed in the art to obtain the styrene butadiene, which is not specifically limited herein. Furthermore, the styrene butadiene in the present invention is synthesized by copolymerizing styrene and butadiene in a molar ratio of (2-8): (2-8).
[0047] Preferably, the mass of the styrene butadiene is 0.5wt%~2wt% of the total mass of the solid phase of the mixed slurry, for example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%.
[0048] In the present invention, if the first binder contains sodium polyacrylate, the solid phase mass of the sodium polyacrylate is 0.8wt%~2wt% of the total solid phase mass of the mixed slurry. For example, it can be 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%.
[0049] According to a preferred embodiment provided by the present invention, the solid content of the mixed slurry is 44wt%~48wt%, for example, it can be 44wt%, 45wt%, 46wt%, 47wt% or 48wt%.
[0050] In a sixth aspect, the present invention provides a battery comprising the negative electrode plate.
[0051] In order to further illustrate the technical solution of the present invention, the present invention provides the following specific embodiments and comparative examples.
[0052] Unless otherwise specified, the various raw materials used in the examples and comparative examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.
[0053] Example 1
[0054] This embodiment provides a PAA binder, and the preparation method thereof comprises the following steps: 50 g of acrylic acid, 12 g of ethylene oxide, 500 g of water, 1 g of ammonium persulfate, 0.6 g of dispersant Hypermer B-246, 0.2 g of sodium dodecyl sulfate, and 0.2 g of polyether silicone Siloxane 2 were added to the reactor, and polymerization was carried out at 90 degrees Celsius and 0.1 MPa. After the reaction, the PAA binder was obtained by neutralization, which was recorded as PAA2. The molecular weight of the PAA2 is 35,000, the viscosity is 15,000 mPas, and the chain segment is branched copolymer (see the schematic diagram). Figure 1 ).
[0055] This embodiment further provides a negative electrode sheet, the preparation method of which includes the following steps: Water, PAA2, styrene butadiene (SBR), sodium polyacrylate (PAA1), sodium carboxymethyl cellulose (CMC) are glued in a double planetary stirring tank for about 2-3 hours, and then hard carbon (HC) is added to obtain a mixed slurry with a solid content of about 44wt%-48wt%, which is then coated on aluminum foil and dried in an oven to obtain a negative electrode sheet. Among them, the mass ratio of HC, CMC, SBR, PAA1 and PAA2 is 96.5%: 0.5%: 1.6%: 1.2%: 0.2%.
[0056] Example 2
[0057] This embodiment provides a negative electrode plate, which is different from Embodiment 1 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA2 is 96.4%:0.5%:1.6%:1.2%:0.3%.
[0058] Example 3
[0059] This embodiment provides a negative electrode plate, which is different from Embodiment 1 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA2 is 96.3%:0.5%:1.6%:1.2%:0.4%.
[0060] Example 4
[0061] This embodiment provides a PAA binder, and the preparation method thereof comprises the following steps: 32 g of acrylic acid, 50 g of ethylene oxide, 500 g of water, 1.5 g of potassium persulfate, 0.6 g of dispersant Hypermer B-246, 0.2 g of sodium dodecyl sulfate, and 0.2 g of polyether silicone Siloxane 2 were added to the reactor, and polymerization was carried out at 90 degrees Celsius and 0.1 MPa. After the reaction, the PAA binder was obtained by neutralization and recorded as PAA3. The molecular weight of the PAA3 is 67,000, the viscosity is 18,000 mPas, and the chain segment is arranged alternately (see the schematic diagram). Figure 2 ).
[0062] This embodiment further provides a negative electrode plate, and the preparation method thereof is different from that of Embodiment 1 only in that PAA2 is replaced by PAA3, and the mass ratio of HC, CMC, SBR, PAA1 and PAA3 is 96.5%:0.5%:1.6%:1.2%:0.2%.
[0063] Example 5
[0064] This embodiment provides a PAA binder, which is different from Embodiment 4 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA3 is 96.4%:0.5%:1.6%:1.2%:0.3%.
[0065] Example 6
[0066] This embodiment provides a PAA binder, which is different from Embodiment 4 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA3 is 96.3%:0.5%:1.6%:1.2%:0.4%.
[0067] Example 7
[0068] This embodiment provides a PAA binder, and the preparation method thereof comprises the following steps: 50 g of acrylic acid, 12 g of acrylonitrile, 500 g of water, 1 g of potassium persulfate, 0.6 g of dispersant Hypermer B-246, 0.2 g of sodium dodecyl sulfate, and 0.2 g of polyether silicone Siloxane 2 were added to a reactor, and a polymerization reaction was carried out at 80 degrees Celsius and 0.1 MPa. After the reaction, the PAA binder was obtained by neutralization and recorded as PAA4. The molecular weight of the PAA4 is 28,000, the viscosity is 8500 mPas, and the segment mode is branched copolymerization.
[0069] This embodiment further provides a negative electrode sheet, and the preparation method thereof is different from that of Embodiment 1 only in that PAA2 is replaced by PAA4, and the mass ratio of HC, CMC, SBR, PAA1 and PAA4 is 96.5%:0.5%:1.6%:1.2%:0.2%.
[0070] Example 8
[0071] This embodiment provides a PAA binder, which is different from Embodiment 7 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA4 is 96.4%:0.5%:1.6%:1.2%:0.3%.
[0072] Example 9
[0073] This embodiment provides a PAA binder, which is different from Embodiment 7 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA4 is 96.3%:0.5%:1.6%:1.2%:0.4%.
[0074] Example 10
[0075] This embodiment provides a PAA binder, and the preparation method thereof comprises the following steps: 20 g of acrylic acid, 50 g of acrylonitrile, 500 g of water, 1.5 g of potassium persulfate, 0.6 g of dispersant Hypermer B-246, 0.2 g of sodium dodecyl sulfate, and 0.2 g of polyether silicone Siloxane 2 were added to a reactor, and a polymerization reaction was carried out at 90 degrees Celsius and 0.1 MPa. After the reaction, the PAA binder was obtained by neutralization and recorded as PAA5. The molecular weight of the PAA5 is 38,000, the viscosity is 12,000 mPas, and the chain segment mode is alternately arranged.
[0076] This embodiment further provides a negative electrode plate, and the preparation method thereof is different from that of Embodiment 1 only in that PAA2 is replaced by PAA5, and the mass ratio of HC, CMC, SBR, PAA1 and PAA5 is 96.5%:0.5%:1.6%:1.2%:0.2%.
[0077] Embodiment 11
[0078] This embodiment provides a PAA binder, which is different from Embodiment 10 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA5 is 96.4%:0.5%:1.6%:1.2%:0.3%.
[0079] Example 12
[0080] This embodiment provides a PAA binder, which is different from Embodiment 10 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA5 is 96.3%:0.5%:1.6%:1.2%:0.3%.
[0081] Embodiment 13
[0082] This embodiment provides a PAA binder, which differs from Embodiment 10 only in that PAA1 is replaced with SBR of equal mass.
[0083] Embodiment 14
[0084] This embodiment provides a PAA binder, which differs from the embodiment 10 only in that acrylic acid is replaced with an equal molar amount of methacrylic acid, and the obtained PAA binder is recorded as PAA6. The molecular weight of the PAA6 is 42,000, the viscosity is 17,000 mPas, and the chain segments are arranged alternately.
[0085] Embodiment 15
[0086] This embodiment provides a negative electrode plate, which is different from Embodiment 1 only in that the mass ratio of HC, CMC, SBR, PAA1 and PAA2 is 96.1%:0.5%:1.6%:1.2%:0.6%.
[0087] Example 16
[0088] This embodiment provides a PAA adhesive, which is different from the embodiment 1 only in that no leveling wetting agent and defoaming agent are added during the reaction.
[0089] Comparative Example 1
[0090] This comparative example provides a negative electrode sheet, which is different from Example 1 only in that the mixed slurry does not contain PAA2, and HC:CMC:SBR:PAA1=96.7%:0.5%:1.6%:1.2%.
[0091] Comparative Example 2
[0092] This comparative example provides a negative electrode plate, which differs from Example 1 only in that PAA2 is replaced by an equal amount of polyethylene oxide (PEO), wherein the molecular weight of the polyethylene oxide is 35,000 to 50,000.
[0093] Comparative Example 3
[0094] This comparative example provides a negative electrode plate, which differs from Example 1 only in that PAA2 is replaced by an equal amount of polyacrylonitrile (PAN), wherein the molecular weight of polyacrylonitrile is 90,000 to 120,000.
[0095] The substances and contents of the solid content of the mixed slurry in the process of preparing the negative electrode sheet in the embodiments and comparative examples are shown in Table 1.
[0096] Table 1
[0097] Test example
[0098] 1. Anti-cracking test: The density of negative electrode sheets after rolling is counted to see how much surface density there is without cracking. In theory, the thicker the thickness, the easier it is to crack.
[0099] The test results are shown in Table 2: Table 2
[0100] 2. Electrochemical performance test
[0101] The present invention further prepares a soft-pack battery using the negative electrode sheets prepared in the embodiment and the comparative example, and the preparation method thereof comprises the following steps: The sodium-ion sodium iron pyrophosphate (NFPP) positive electrode sheet with a single-sided surface density of 130 g / m2, the 9-micron (PE layer) + 3-micron (ceramic layer) + 1-micron (glue layer) composite separator, and the prepared negative electrode sheet are stacked in order so that the separator is between the positive and negative electrode sheets, and the stacking is performed to obtain a bare battery cell; the bare battery cell is placed in an aluminum-plastic film outer packaging, vacuum dried at 85 degrees Celsius, and the above-prepared electrolyte is injected into the dried battery after the moisture meets the standard, and the battery is packaged, allowed to stand, formed, and divided to complete the preparation of the sodium-ion battery.
[0102] Relevant performance tests were performed on the above-mentioned sodium ion batteries and their electrolytes.
[0103] 2.1 Cycle performance test: Place the sodium ion battery in a 25 degree Celsius constant temperature chamber and a 45 degree Celsius constant temperature chamber respectively, and let it stand for 30 minutes to allow the sodium ion battery to reach a constant temperature. The sodium ion battery that has reached a constant temperature is charged at a constant current of 1C to 4.0V, then charged at a constant voltage until the current drops to 0.05C, and then discharged at a constant current of 1C to 1.5V. This cycle is repeated, and the discharge capacity of the first cycle and the discharge capacity of the last cycle are recorded. The capacity retention rate is calculated according to the following formula.
[0104] Cycle capacity retention rate at the Xth cycle (%) = (discharge capacity at the Xth cycle / discharge capacity at the first cycle) × 100%
[0105] 3) DCR test: Take a fresh cell with 50% SOC and discharge it at a given current of 1C for 360s (100ms sampling point).
[0106] DCR calculation = (discharge initial voltage - battery voltage at 1C discharge for 360s) / 1.0C × 1000
[0107] In this system, 1C=2A
[0108] 2.2 Electrical performance test: The test results are shown in Table 3: Table 3
[0109] The results show that the alternatingly arranged PAA has a better anti-cracking effect and better electrochemical performance than the branched copolymer PAA; according to Example 13 compared with Example 12, it can be seen that when the binder composition is a mixture of PAA binder, sodium polyacrylate and styrene butadiene, the electrode processing performance and the electrochemical performance of the battery are better than the mixture of PAA binder and any one. According to Example 14 compared with other examples, when the first monomer selects one or more of the acrylate, methacrylic acid, methacrylate, propylene sulfonic acid, propylene sulfonate, methacrylic acid, methacrylic acid, itaconic acid, itaconic acid, maleic acid and maleate defined in the present invention, it has an effect equivalent to acrylic acid. Due to space limitations, the present invention does not give examples one by one. According to Example 15 compared with Example 1, when the amount of PAA binder in the mixed slurry is higher than 0.4wt%, it will affect the processing performance of the electrode and the electrochemical performance of the battery. According to Example 16 compared with Example 1, it can be seen that when the leveling wetting agent and defoaming agent are not added during the preparation of the PAA binder, the processing performance of the pole piece and the electrochemical performance of the battery will also be affected. According to Comparative Example 1 compared with the example, when the PAA binder described in the present application is not added, the processing performance of the pole piece is poor, cracking will occur when the surface density is 90 grams / square meter, and the electrochemical performance of the battery is also poor; this shows that the synthesis of the sodium negative electrode binder at the molecular level can avoid problems such as uneven distribution of various parts, especially the combination of soft and hard ensures that it has good processability in thick electrodes. According to Comparative Examples 2 to 3 compared with the example, even if polyethylene oxide or polyacrylonitrile is added to the mixed slurry, the processing performance of the pole piece is poor, and it also has a great impact on the electrochemical performance of the battery.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A PAA binder, characterized in that: It is obtained by copolymerizing a first monomer and a second monomer, wherein the first monomer and the second monomer form a segment in a branched copolymerization or alternating arrangement manner; The first monomer is an unsaturated acid or an unsaturated acid salt, and the second monomer is ethylene oxide or acrylonitrile.
2. The PAA binder according to claim 1, characterized in that: The molecular weight of the PAA binder is 10,000 to 200,000; and / or the viscosity of the PAA binder is 5,000 to 20,000 mPas.
3. The PAA binder according to claim 1, characterized in that: The first monomer includes one or more of acrylic acid, acrylic acid salt, methacrylic acid, methacrylic acid salt, propylene sulfonic acid, propylene sulfonate, methacrylic acid, methacrylic acid sulfonate, itaconic acid, itaconic acid salt, maleic acid and maleate salt; preferably acrylic acid.
4. The PAA binder according to claim 1, characterized in that: The molar ratio of the first monomer to the second monomer is (2-8): (2-8); Preferably, when the molar ratio of the first monomer to the second monomer is (6-8): (2-4), the PAA binder forms a branched copolymer structure; when the molar ratio of the first monomer to the second monomer is (2-4): (6-8), the PAA binder forms an alternating structure.
5. The method for preparing the PAA binder according to any one of claims 1 to 4, characterized in that: include: The first monomer, the second monomer, the first solvent and the initiator are mixed, and a polymerization reaction is carried out at 40-100 degrees Celsius and 0.1-1 MPa; preferably, the first solvent includes water, and the initiator includes one or more of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and benzoyl peroxide.
6. The method for preparing the PAA binder according to claim 5, characterized in that: The preparation method of the PAA binder comprises: mixing the first monomer, the second monomer, the first solvent, the first dispersant, the leveling wetting agent, the defoaming agent and the initiator, and performing a polymerization reaction at 40-100 degrees Celsius and 0.1-1 MPa; more preferably, the first dispersant comprises water, the leveling wetting agent comprises one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium secondary alkyl sulfonate and sodium α-olefin sulfonate, and the defoaming agent comprises one or more of polyether silicone, gemini glycol polyether and star polyether.
7. A binder composition, characterized in that: It comprises the PAA binder according to any one of claims 1 to 4 and a first binder; the first binder comprises sodium polyacrylate and / or styrene butadiene.
8. A negative electrode plate, characterized in that: Contains the PAA binder according to any one of claims 1 to 4 or the binder composition according to claim 7.
9. The method for preparing the negative electrode sheet according to claim 8, characterized in that: include: The sodium negative electrode active material, the binder composition according to claim 7, the second dispersant and the second solvent are mixed, the obtained mixed slurry is coated on the current collector, and then dried to obtain the negative electrode sheet; the binder composition comprises the PAA binder according to any one of claims 1 to 4 and the first binder; Preferably, the mass of the PAA binder is 0.2wt%-0.6wt% of the total mass of the solid phase of the mixed slurry.
10. A battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet according to claim 8.
Citation Information
Patent Citations
Sodium battery negative electrode binder, sodium battery negative electrode plate and sodium ion battery
CN118016893A