Low-temperature foaming heat-reduced adhesive glue, adhesive film and preparation method
By combining the formula acrylate adhesive with foamed microspheres, low-temperature foaming heat-reducing glue and adhesive film were prepared, which solved the deformation and precipitation problems of existing heat-reducing tapes when they were unbonded at high temperatures. , realizes rapid detachment and shedding of products at low temperatures and efficient heat transfer.
Patent Information
- Application Number
- CN202411041941.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When existing heat-relieving tapes are unbonded at high temperatures, they lead to problems such as temperature-resistant product deformation, additive precipitation, and small molecules precipitation, and low heat transfer efficiency, which cannot meet the process requirements of rapid debonding at low temperatures.
Using low-temperature foaming heat-reducing glue and adhesive film, the formulation components are optimized, including the combination of acrylic adhesive, foamed microspheres and curing agents, to prepare a cutting that can be initially sticky and high at room temperature and 60℃. It still has good viscosity and completely loses stickiness and does not leave glue at low temperatures of 80-100℃.
It realizes rapid detachment and fall off of products under low temperature conditions, avoids deformation and precipitation problems caused by high temperature, improves heat transfer efficiency, and is suitable for the production process of high-temperature products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of viscosity-reducing adhesive materials, and in particular to a low-temperature foaming thermal viscosity-reducing adhesive, an adhesive film and a preparation method thereof. Background Art
[0002] Viscosity-reducing adhesive is a new type of adhesive material that can temporarily fix and protect the surface of the product to prevent mechanical scratches, wear, pollution and corrosion. When fixation or protection is not needed, it is stimulated by certain effects such as ultraviolet light viscosity reduction, thermal viscosity reduction or electrical, magnetic, and ultrasonic stimulation, so that it can be easily separated from the surface of the adherend without damaging the product. On the one hand, the thermal viscosity-reducing protective film requires extremely high adhesion to ensure the stability of the initial back sticker, and on the other hand, it requires that there is basically no residual glue or broken glue on the surface after heat treatment, so as to ensure the subsequent process. That is, it has a certain adhesion at room temperature, and as long as it is heated to the set temperature, the adhesion disappears, which can achieve easy peeling, no residual glue, and no pollution to the adherend. In the production process of chip electronic components, spare parts and other products, because some parts are not resistant to high temperatures, and in order to meet the needs of efficient operation, a thermal debonding tape that can quickly debond and fall off at low temperatures is needed. However, most of the thermal debonding tapes on the market currently require high temperatures above 100°C to completely debond. Some products are not heat-resistant during the process. If the debonding temperature is too high, it will cause product deformation, precipitation of additives, precipitation of small molecules and other problems. In addition, the heat transfer efficiency and time of the heating equipment during thermal debonding are different. When the process requires a low thermal debonding temperature and debonding in equipment with low heat transfer efficiency (such as an oven), ordinary thermal debonding adhesives cannot meet the process requirements.
[0003] At present, when temporarily fixing and protecting products, most thermal debonding tapes have high thermal debonding temperatures. However, thermal debonding tapes with high temperature debonding are not suitable for plastic parts that are not resistant to high temperatures and different manufacturing processes. For example, patent CN113817423A invented a thermal debonding film with a debonding temperature of 100-200°C and a method for preparing the same. CN113416497A invented a segmented thermal debonding protective film that loses part of its viscosity at 100°C and can almost completely debond at 140°C. Patent CN106433506A discloses a heated debonding protective film and a method for preparing the same, with a debonding temperature of 160°C. After debonding, the film automatically peels off without residual glue. Patent CN115926691A discloses a thermal debonding tape that can be completely peeled off from the back sticker without residual glue after heating at 140°C for 10 minutes. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a low-temperature foaming heat-reducing viscosity-reducing glue, a glue film and a preparation method thereof in view of the deficiencies in the above-mentioned prior art.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: in the first aspect of the present invention, a low-temperature foaming heat-reducing viscosity-reducing glue is provided, comprising the following raw material components in parts by weight:
[0006] 80-100 parts of acrylic adhesive;
[0007] 1-3 parts of curing agent;
[0008] 25-50 parts of the first solvent;
[0009] 3-7 parts of foamed microspheres;
[0010] Among them, the mass ratio of curing agent: foamed microspheres is 1:1.5 to 1:2.2.
[0011] Preferably, the foaming microspheres are selected from one or more of the following products: 031DU40, 051DU40 and 093DU120 foaming microspheres produced by Akzo Nobel High Performance Chemicals Co., Ltd., and F-36D, HF-36D, F-36LVD, HF-48D, F-65D and F-82D foaming microspheres produced by Matsumoto Oil Pharmaceutical Co., Ltd.
[0012] Preferably, the curing agent is selected from one or more of an isocyanate curing agent, a peroxide curing agent and an epoxy curing agent;
[0013] The first solvent is selected from one or more of ethyl acetate, toluene, acetylacetone, butanone and isopropanol.
[0014] Preferably, the acrylic adhesive comprises the following raw material components in parts by weight:
[0015] 5-20 parts of hard monomer;
[0016] Soft monomer 20-50 parts;
[0017] 1-5 parts of cross-linking monomer;
[0018] Initiator 0.1-1 part;
[0019] The second solvent is 100-120 parts.
[0020] Preferably, the hard monomer is selected from one or more of styrene, acrylonitrile, vinyl acetate, and methyl methacrylate;
[0021] The soft monomer is selected from one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, and lauryl acrylate;
[0022] The cross-linking monomer is selected from one or more of acrylic acid, methacrylic acid, N-hydroxymethyl acrylamide, and hydroxyethyl acrylate.
[0023] Preferably, the initiator is selected from one or more of benzoyl peroxide, dodecyl peroxide, di-tert-butyl peroxide, azobisisobutyronitrile, dimethyl azobisisobutyrate, azobisisoheptanenitrile, and cumene hydroperoxide;
[0024] The second solvent is selected from one or more of ethyl acetate, toluene, acetone and isopropanol.
[0025] Preferably, the hard monomer is styrene, the soft monomer is a mixture of ethyl acrylate and isooctyl acrylate, and the cross-linking monomer is acrylic acid.
[0026] Preferably, the acrylic adhesive is prepared by the following method:
[0027] The hard monomer, the soft monomer, the cross-linking monomer and part of the second solvent are mixed, and stirred for 5-30 minutes under nitrogen filling, and then part of the initiator is added, and the remaining initiator and the remaining solvent are added after stirring and reacting at 70-78° C. for 1.5-6 hours, and the stirring reaction is continued at 70-78° C. for 1-4 hours, and then the temperature is lowered to below 30° C., and the material is discharged to obtain the acrylic adhesive.
[0028] The second aspect of the present invention provides a method for preparing the low-temperature foaming heat-reducing viscosity-reducing glue as described above, comprising the following steps:
[0029] S1. Dispersion treatment of foamed particles:
[0030] According to the mass ratio of foaming microspheres to the first solvent of 1:2 to 1:5, 4 to 6 parts by weight of the foaming microspheres are added to a portion of the first solvent under stirring at a speed of 2000 to 3500 rpm / min, and stirring is continued for 10 to 20 minutes to obtain a foamed particle dispersion;
[0031] S2, adding the foamed particle dispersion obtained in step S1 and the remaining part of the first solvent to 80-100 parts by weight of the acrylic adhesive, continuing to stir at a speed greater than 600 rpm / min for 10-20 min, adding 2-3 parts by weight of a curing agent under continuous stirring, continuing to stir for 20-30 min, filtering with 200-300 mesh gauze, discarding the filter residue, and then standing for 0.5-2 hours to defoam, to obtain the low-temperature foaming heat-reducing viscosity-reducing glue.
[0032] The third aspect of the present invention provides a low-temperature foaming heat-reducing adhesive film, which is prepared by the following method:
[0033] The low-temperature foaming heat-reducing adhesive as described above is evenly coated on the substrate, the dry adhesive thickness is controlled to be 50-60 μm, baked at 70-80° C. for 3-5 minutes, cooled to room temperature, and then covered with a release film on the adhesive surface, and then aged at 50-60° C. for 2-4 days to obtain the low-temperature foaming heat-reducing adhesive film.
[0034] The beneficial effects of the present invention are:
[0035] The present invention prepares an acrylate adhesive with appropriate initial adhesion and cohesive force and suitable for heat-reducing viscosity film by optimizing the formula components, and compounding the acrylate adhesive with foaming microspheres and a curing agent to obtain a low-temperature foaming heat-reducing viscosity glue and film that can be applied to temperature-sensitive products. The acrylate adhesive can achieve high initial adhesion at room temperature, and the product still has good adhesion when cut at 60°C. It can completely lose adhesion without leaving any glue when heated at a low temperature of 80-100°C, and has good market application prospects. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0037] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0038] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0039] The present invention provides a low-temperature foaming heat-reducing viscosity-reducing glue, comprising the following raw material components in parts by weight:
[0040] 80-100 parts of acrylic adhesive;
[0041] 1-3 parts of curing agent;
[0042] 25-50 parts of the first solvent;
[0043] 3-7 parts of foamed microspheres.
[0044] Among them, the mass ratio of curing agent: foamed microspheres is 1:1.5 to 1:2.2.
[0045] The amount of curing agent used greatly affects the viscosity of the thermal anti-viscosity film. The amount of foamed microspheres used also greatly affects whether the thermal anti-viscosity film can completely lose viscosity at low temperatures. The added curing agent and foamed microspheres need to be controlled within a suitable ratio range to ensure that the thermal anti-viscosity film can adhere to the product without falling off during the cutting process of subsequent applications, and can achieve complete loss of viscosity without leaving any glue during thermal loss of viscosity.
[0046] The foaming microspheres should have good expansibility, and the shape has certain stability under continuous high temperature environment, and can still maintain a good expanded state without shrinking. The foaming microspheres are usually shell-shaped polymers containing low-boiling alkane liquids, which are gasified and expanded after being heated. According to the foaming temperature requirements, in a preferred embodiment, the foaming microspheres are selected from one or more of the following products: 031DU40, 051DU40 and 093DU120 foaming microspheres produced by Akzo Nobel High-Efficiency Chemicals Co., Ltd., and F-36D, HF-36D, F-36LVD, HF-48D, F-65D and F-82D foaming microspheres produced by Matsumoto Oil Pharmaceutical Co., Ltd.
[0047] In a preferred embodiment, the curing agent is selected from one or more of an isocyanate curing agent, a peroxide curing agent, and an epoxy curing agent. If the amount of curing agent used is too much, the initial adhesion and steel plate force of the tape are low, and it is not possible to fit the object well, and play a good fixing and protective role. If the amount of curing agent used is too little, the normal temperature and high temperature steel plate force of the tape are high, which affects the thermal debonding effect and rate. In the present invention, the addition amount is preferably 2-3 parts by weight. Increasing the amount of foamed microspheres and curing agent added can reduce the normal temperature steel plate force of the thermal debonding film, which helps the thermal debonding film to completely debond in a wider low temperature range, but excessive foamed microspheres will also reduce the high temperature steel plate force and reduce the adhesion to the object at high temperature.
[0048] In a preferred embodiment, the first solvent is selected from one or more of ethyl acetate, toluene, acetylacetone, butanone and isopropanol.
[0049] In a preferred embodiment, the acrylic adhesive comprises the following raw material components in parts by weight:
[0050] 5-20 parts of hard monomer;
[0051] Soft monomer 20-50 parts;
[0052] 1-5 parts of cross-linking monomer;
[0053] Initiator 0.1-1 part;
[0054] The second solvent is 100-120 parts.
[0055] In a preferred embodiment, the hard monomer is selected from one or more of styrene, acrylonitrile, vinyl acetate, and methyl methacrylate;
[0056] In a preferred embodiment, the soft monomer is selected from one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, and lauryl acrylate;
[0057] In a preferred embodiment, the crosslinking monomer is selected from one or more of acrylic acid, methacrylic acid, N-hydroxymethyl acrylamide, and hydroxyethyl acrylate.
[0058] In a preferred embodiment, the initiator is selected from one or more of benzoyl peroxide, dodecyl peroxide, di-tert-butyl peroxide, azobisisobutyronitrile, dimethyl azobisisobutyrate, azobisisoheptanenitrile, and cumene hydroperoxide;
[0059] In a preferred embodiment, the second solvent is selected from one or more of ethyl acetate, toluene, acetone and isopropanol.
[0060] In a more preferred embodiment, the hard monomer is styrene, the soft monomer is a mixture of ethyl acrylate and isooctyl acrylate, and the crosslinking monomer is acrylic acid.
[0061] In a preferred embodiment, the acrylic adhesive is prepared by the following method:
[0062] The hard monomer, soft monomer, cross-linking monomer and part of the second solvent are mixed, and stirred for 5-30 minutes under nitrogen. Then part of the initiator is added, and the stirring reaction is carried out at 70-78° C. for 1.5-6 hours, and then the remaining initiator and the remaining solvent are added. The stirring reaction is continued at 70-78° C. for 1-4 hours, and then the temperature is lowered to below 30° C., and the material is discharged to obtain an acrylic adhesive.
[0063] The present invention also provides a method for preparing the above low-temperature foaming heat-reducing viscosity-reducing glue, comprising the following steps:
[0064] S1. Dispersion treatment of foamed particles:
[0065] According to the mass ratio of the foaming microspheres to the first solvent of 1:2 to 1:5, 4 to 6 parts by weight of the foaming microspheres are added to a portion of the first solvent under stirring at a speed of 2000 to 3500 rpm / min, and care is taken to prevent the foamed particles from agglomerating. After all the foamed particles are added, the container is sealed and stirred for 10 to 20 minutes to obtain a foamed particle dispersion;
[0066] S2, adding the foamed particle dispersion obtained in step S1 and the remaining part of the first solvent to 80-100 parts by weight of the acrylic adhesive, continuing to stir at a speed greater than 600 rpm / min for 10-20 min, adding 2-3 parts by weight of a curing agent under continuous stirring, continuing to stir for 20-30 min, filtering with 200-300 mesh gauze, discarding the filter residue, and then standing for 0.5-2 hours to defoam, to obtain a low-temperature foaming thermal viscosity-reducing glue.
[0067] The present invention also provides a low-temperature foaming heat-reducing adhesive film, which is prepared by the following method:
[0068] The low-temperature foaming heat-reducing adhesive is evenly coated on the substrate, the dry adhesive thickness is controlled to be 50-60 μm, baked at 70-80°C for 3-5 minutes, cooled to room temperature, and then covered with a release film on the adhesive surface, and then aged at 50-60°C for 2-4 days to obtain a low-temperature foaming heat-reducing adhesive film.
[0069] The release film is used as a protective material for the adhesive layer. It will be peeled off from the adhesive layer and discarded during subsequent use. It does not belong to the use layer. When selecting, the appropriate peeling force and release force must be considered. One of the base material release films such as PE, PP, PET, etc. can be selected, and the thickness is generally 20-70μm.
[0070] Since foamed particles are dispersed in the adhesive layer, in order to ensure that the foamed particles can be evenly dispersed in the adhesive layer and the heat-reduced adhesive tape has a higher initial adhesion and steel plate strength, the thickness of the adhesive layer is generally greater than 50μm.
[0071] The substrate serves as the supporting substrate of the heat-reducing viscosity film, and various types of substrates may be selected, such as plastic, metal foil, high temperature resistant paper and non-woven fabric. The plastic substrate may be selected from one of the base films such as PET, PP, PE, BOPP, PC, PVC, PO, etc. For example, a PET base film may be selected, and its thickness is generally 60-120μm.
[0072] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0073] Example 1 Acrylic Adhesive Optimization Experiment
[0074] 1-1. Use the following method to synthesize acrylic adhesive:
[0075] 50 parts of soft monomers ethyl acrylate and isooctyl acrylate, 5 parts of hard monomers styrene and 2 parts of cross-linking monomers acrylic acid, and 100 parts of solvent ethyl acetate were added into a four-necked flask equipped with a stirring paddle, a reflux condenser and a nitrogen inlet tube. Nitrogen was filled into the reaction flask and stirred thoroughly for 10 minutes. Then 0.3 parts of initiator benzoyl peroxide was added, and after reacting at 75°C for 3 hours, the remaining 0.1 parts of benzoyl peroxide and 20 parts of ethyl acetate were added, and the reaction was continued at 75°C with stirring for 2 hours. The temperature was cooled to room temperature, and the acrylic adhesive was obtained.
[0076] 1-2. Use the following method to synthesize acrylic adhesive:
[0077] 45 parts of soft monomers ethyl acrylate, isooctyl acrylate, 10 parts of hard monomers styrene, 2 parts of cross-linking monomers acrylic acid, and 100 parts of solvent ethyl acetate were added into a four-necked flask equipped with a stirring paddle, a reflux condenser, and a nitrogen inlet tube. Nitrogen was filled into the reaction flask and stirred for 10 minutes. Then 0.3 parts of initiator benzoyl peroxide was added. After reacting at 75°C for 3 hours, the remaining 0.1 parts of benzoyl peroxide and 20 parts of ethyl acetate were added, and the reaction was continued at 75°C with stirring for 2 hours. The temperature was cooled to room temperature, and the acrylic adhesive was obtained.
[0078] 1-3. Use the following method to synthesize acrylic adhesive:
[0079] 40 parts of soft monomers ethyl acrylate, isooctyl acrylate, 15 parts of hard monomers styrene, 2 parts of cross-linking monomers acrylic acid, and 100 parts of solvent ethyl acetate were added into a four-necked flask equipped with a stirring paddle, a reflux condenser, and a nitrogen inlet tube. Nitrogen was filled into the reaction flask and stirred for 10 minutes. Then 0.3 parts of initiator benzoyl peroxide was added. After reacting at 75°C for 3 hours, the remaining 0.1 parts of benzoyl peroxide and 20 parts of ethyl acetate were added, and the reaction was continued at 75°C with stirring for 2 hours. The temperature was cooled to room temperature, and the acrylic adhesive was obtained.
[0080] 1-4. Use the following method to synthesize acrylic adhesive:
[0081] 30 parts of soft monomers ethyl acrylate, isooctyl acrylate, 15 parts of hard monomers styrene, 2 parts of cross-linking monomers acrylic acid, and 100 parts of solvent ethyl acetate were added into a four-necked flask equipped with a stirring paddle, a reflux condenser, and a nitrogen inlet tube. Nitrogen was filled into the reaction flask and stirred for 10 minutes. Then 0.3 parts of initiator benzoyl peroxide was added. After reacting at 75°C for 3 hours, the remaining 0.1 parts of benzoyl peroxide and 20 parts of ethyl acetate were added, and the reaction was continued at 75°C with stirring for 2 hours. The temperature was cooled to room temperature, and the acrylic adhesive was obtained.
[0082] Performance Test:
[0083] Each acrylate adhesive was coated on a PET substrate, baked at 75°C for 4 min, supported on a tape sample, and then subjected to the following performance tests.
[0084] (1) Steel plate force at room temperature (gf / inch), using a tensile testing machine, model: KJ-1065B, tested according to ASTM 3330;
[0085] (2) 60℃ steel plate force (gf / inch), using a double-arm tensile testing machine, model: 3360, tested according to ASTM 3330;
[0086] (3) The test method for residual glue is:
[0087] The sample is 25 mm wide and 170 mm long. It is attached to a clean ceramic sheet (100 mm*150 mm) and rolled back and forth twice with a 2KG roller. After standing for 20 minutes, it is peeled off at an angle of 180° at a speed of 300 mm / min using a tensile testing machine to observe the surface of the ceramic sheet.
[0088] The test results are shown in Table 1 below:
[0089] Table 1
[0090]
[0091] According to the test results in Table 1, the Tg of the soft monomer is lower than -20°C. When the amount of soft monomer added is low, the viscosity of the polymer is low. When it is too high, the polymer cohesion is poor. When the amount of hard monomer added is too low, the polymer cohesion is poor, and the shear resistance is extremely poor at high temperature. When it is too high, the polymer viscosity is low. Acrylic adhesives are also required to have excellent initial adhesion and lasting adhesion at room temperature. Appropriate cohesion can effectively reduce residual glue and effectively reduce peeling force after heating, and play a role in thermal viscosity reduction in the subsequent high-temperature foaming of thermal debonding film. Based on the subsequent preparation of low-temperature thermal debonding film, the initial viscosity and cohesion of acrylic adhesives and the subsequent process of low-temperature thermal debonding film obtained by adding foamed particles are comprehensively considered, and the acrylic adhesives prepared by the methods of Examples 1-3 are used in subsequent examples and comparative examples.
[0092] Example 2
[0093] A low-temperature foaming heat-reducing adhesive film is prepared by the following method:
[0094] S1. Dispersion treatment of foamed particles:
[0095] 5 parts by weight of foamed microspheres (031DU40 foamed microspheres produced by Akzo Nobel High-Efficiency Chemicals Co., Ltd.) were added to 25 parts by weight of the first solvent (ethyl acetate) under stirring at a speed of 3000 rpm / min, and care was taken to prevent the foamed particles from agglomerating. After all the foamed particles were added, the container was sealed and stirred for 15 minutes to obtain a foamed particle dispersion;
[0096] S2. Add the foamed particle dispersion obtained in step S1 and 25 parts by weight of the first solvent (ethyl acetate) to 100 parts by weight of the acrylic adhesive, continue stirring at a speed of 1000 rpm / min for 15 minutes, add 3 parts by weight of a curing agent (specifically Wanhua Chemical HT-100) under continuous stirring, continue stirring for 30 minutes, filter with 200-mesh gauze, discard the filter residue, and then stand for 1 hour to defoam, to obtain the low-temperature foaming thermal viscosity-reducing glue.
[0097] S3. Evenly apply the low-temperature foaming heat-reducing adhesive on a PET substrate with a thickness of 100 μm, control the dry adhesive thickness to 55 μm, bake at 75°C for 4 minutes, cool to room temperature, and then cover the adhesive surface with a 20 μm release film, and then mature at 60°C-50°C for 3 days to obtain the low-temperature foaming heat-reducing adhesive film.
[0098] Comparative Example 1
[0099] A low-temperature foaming heat-reducing adhesive film is prepared by the following method:
[0100] S1. Dispersion treatment of foamed particles:
[0101] 3 parts by weight of foamed microspheres (031DU40 foamed microspheres produced by Akzo Nobel High-Efficiency Chemicals Co., Ltd.) were added to 15 parts by weight of the first solvent (ethyl acetate) under stirring at a speed of 1500 rpm / min, and care was taken to prevent the foamed particles from agglomerating. After all the foamed particles were added, the container was sealed and stirred for 15 minutes to obtain a foamed particle dispersion;
[0102] S2. Add the foamed particle dispersion obtained in step S1 and 35 parts by weight of the first solvent (ethyl acetate) to 100 parts by weight of the acrylic adhesive, continue stirring at a speed of 1000 rpm / min for 15 minutes, add 1 part by weight of a curing agent (specifically Wanhua Chemical HT-100) under continuous stirring, continue stirring for 30 minutes, filter with 200-mesh gauze, discard the filter residue, and then stand for 1 hour to defoam, to obtain the low-temperature foaming thermal viscosity-reducing glue.
[0103] S3. Evenly apply the low-temperature foaming heat-reducing adhesive on a PET substrate with a thickness of 100 μm, control the dry adhesive thickness to 55 μm, bake at 75°C for 4 minutes, cool to room temperature, and then cover the adhesive surface with a 20 μm release film, and then mature at 50°C for 3 days to obtain the low-temperature foaming heat-reducing adhesive film.
[0104] Comparative Example 2
[0105] A low-temperature foaming heat-reducing adhesive film is prepared by the following method:
[0106] S1. Dispersion treatment of foamed particles:
[0107] 3 parts by weight of foamed microspheres (031DU40 foamed microspheres produced by Akzo Nobel High-Efficiency Chemicals Co., Ltd.) were added to 15 parts by weight of the first solvent (ethyl acetate) under stirring at a speed of 3000 rpm / min, and care was taken to prevent the foamed particles from agglomerating. After all the foamed particles were added, the container was sealed and stirred for 15 minutes to obtain a foamed particle dispersion;
[0108] S2. Add the foamed particle dispersion obtained in step S1 and 35 parts by weight of the first solvent (ethyl acetate) to 100 parts by weight of the acrylic adhesive, continue stirring at a speed of 1000 rpm / min for 15 minutes, add 1 part by weight of a curing agent (specifically Wanhua Chemical HT-100) under continuous stirring, continue stirring for 30 minutes, filter with 200-mesh gauze, discard the filter residue, and then stand for 1 hour to defoam, to obtain the low-temperature foaming thermal viscosity-reducing glue.
[0109] S3. Evenly apply the low-temperature foaming heat-reducing adhesive on a PET substrate with a thickness of 100 μm, control the dry adhesive thickness to 55 μm, bake at 75°C for 4 minutes, cool to room temperature, and then cover the adhesive surface with a 20 μm release film, and then mature at 50°C for 3 days to obtain the low-temperature foaming heat-reducing adhesive film.
[0110] Comparative Example 3
[0111] A low-temperature foaming heat-reducing adhesive film is prepared by the following method:
[0112] S1. Dispersion treatment of foamed particles:
[0113] 7 parts by weight of foamed microspheres (031DU40 foamed microspheres produced by Akzo Nobel High-Efficiency Chemicals Co., Ltd.) were added to 35 parts by weight of the first solvent (ethyl acetate) under stirring at a speed of 3000 rpm / min, and care was taken to prevent the foamed particles from agglomerating. After all the foamed particles were added, the container was sealed and stirred for 15 minutes to obtain a foamed particle dispersion;
[0114] S2. Add the foamed particle dispersion obtained in step S1 and 15 parts by weight of the first solvent (ethyl acetate) to 100 parts by weight of the acrylic adhesive, continue stirring at a speed of 1000 rpm / min for 15 minutes, add 3 parts by weight of a curing agent (specifically Wanhua Chemical HT-100) under continuous stirring, continue stirring for 30 minutes, filter with 200-mesh gauze, discard the filter residue, and then stand for 1 hour to defoam, to obtain the low-temperature foaming thermal viscosity-reducing glue.
[0115] S3. Evenly apply the low-temperature foaming heat-reducing adhesive on a PET substrate with a thickness of 100 μm, control the dry adhesive thickness to 55 μm, bake at 75°C for 4 minutes, cool to room temperature, and then cover the adhesive surface with a 20 μm release film, and then mature at 50°C for 3 days to obtain the low-temperature foaming heat-reducing adhesive film.
[0116] The following performance tests were performed on the low-temperature foaming heat-reducing adhesive films prepared in Example 2 and Comparative Examples 1-3:
[0117] 1. Steel plate force at room temperature (gf / inch), using a tensile testing machine, model: KJ-1065B, tested according to ASTM 3330 standard;
[0118] 2. High temperature steel plate force (gf / inch), using a double-arm tensile machine, model: 3360, tested according to ASTM 3330 standard;
[0119] 3. 60℃ cutting state, the test method is:
[0120] Put a 100mm*100mm sample on a clean ceramic plate (100mm*100mm), put it into a 60℃ constant temperature air drying oven or electric heating plate with the sample at the bottom and the ceramic plate at the top, keep it there for 5 minutes, take it out, and observe whether the sample is tightly attached to the ceramic plate after cooling.
[0121] 4. For the viscosity loss at 75℃, 85℃ and 95℃, use a constant temperature air drying oven and an electric heating plate to heat to the corresponding temperature and observe the viscosity loss.
[0122] The test results are shown in Table 2 below:
[0123] Table 2
[0124]
[0125]
[0126] According to the test results in Table 2, the expanded particles in Example 2 are evenly dispersed and have suitable adhesion at room temperature and a temperature not greater than 75°C, while the adhesion decreases after heating, and the effect of complete viscosity reduction can be achieved under low temperature heating (80°C-100°C).
[0127] In Comparative Examples 1 and 2, the amount of foamed microspheres added is too small, and the viscosity reduction effect of low-temperature heating (85-95°C) cannot be achieved; and the rotation speed for preparing the foamed microsphere dispersion in Comparative Example 1 is too low, and there is a phenomenon of uneven dispersion of the foamed microspheres; in Comparative Example 3, the amount of foamed microspheres added is too large, resulting in too low adhesion at room temperature and low temperature (not more than 75°C).
[0128] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A low-temperature foaming heat-reducing adhesive, characterized in that: The invention comprises the following raw material components by weight: 80-100 parts of acrylic adhesive; 1-3 parts of curing agent; 25-50 parts of the first solvent; 3-7 parts of foamed microspheres; Among them, the mass ratio of curing agent: foamed microspheres is 1:1.5 to 1:2.
2.
2. The low-temperature foaming heat-reducing viscosity-reducing glue according to claim 1, characterized in that: The foaming microspheres are selected from one or more of the following products: 031DU40, 051DU40 and 093DU120 foaming microspheres produced by Akzo Nobel High Performance Chemicals Co., Ltd., and F-36D, HF-36D, F-36LVD, HF-48D, F-65D and F-82D foaming microspheres produced by Matsumoto Oil Pharmaceutical Co., Ltd.
3. The low-temperature foaming heat-reducing viscosity-reducing glue according to claim 1, characterized in that: The curing agent is selected from one or more of an isocyanate curing agent, a peroxide curing agent and an epoxy curing agent; The first solvent is selected from one or more of ethyl acetate, toluene, acetylacetone, butanone and isopropanol.
4. The low-temperature foaming heat-reducing adhesive according to claim 1, characterized in that: The acrylic adhesive comprises the following raw material components by weight: 5-20 parts of hard monomer; Soft monomer 20-50 parts; 1-5 parts of cross-linking monomer; Initiator 0.1-1 part; The second solvent is 100-120 parts.
5. The low-temperature foaming heat-reducing adhesive according to claim 4, characterized in that: The hard monomer is selected from one or more of styrene, acrylonitrile, vinyl acetate, and methyl methacrylate; the soft monomer is selected from one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, and lauryl acrylate; The cross-linking monomer is selected from one or more of acrylic acid, methacrylic acid, N-hydroxymethyl acrylamide, and hydroxyethyl acrylate.
6. The low-temperature foaming heat-reducing viscosity-reducing glue according to claim 4, characterized in that: The initiator is selected from one or more of benzoyl peroxide, dodecyl peroxide, di-tert-butyl peroxide, azobisisobutyronitrile, dimethyl azobisisobutyrate, azobisisoheptanenitrile, and cumene hydroperoxide; The second solvent is selected from one or more of ethyl acetate, toluene, acetone and isopropanol.
7. The low-temperature foaming heat-reducing adhesive according to claim 5, characterized in that: The hard monomer is styrene, the soft monomer is a mixture of ethyl acrylate and isooctyl acrylate, and the cross-linking monomer is acrylic acid.
8. The low-temperature foaming heat-reducing adhesive according to claim 4, characterized in that: The acrylic adhesive is prepared by the following method: The hard monomer, the soft monomer, the cross-linking monomer and part of the second solvent are mixed, and stirred for 5-30 minutes under nitrogen, and then part of the initiator is added, and the stirring reaction is continued at 70-78° C. for 1.5-6 hours, and then the remaining initiator and the remaining solvent are added, and the stirring reaction is continued at 70-78° C. for 1-4 hours, and then the temperature is lowered to below 30° C., and the material is discharged to obtain the acrylic adhesive.
9. A method for preparing the low-temperature foaming heat-reducing adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Dispersion treatment of foamed particles: According to the mass ratio of the foaming microspheres to the first solvent being 1:2 to 1:5, 4 to 6 parts by weight of the foaming microspheres are added to a portion of the first solvent under stirring at a speed of 2000 to 3500 rpm / min, and stirring is continued for 10 to 20 minutes to obtain a foamed particle dispersion; S2, adding the foamed particle dispersion obtained in step S1 and the remaining part of the first solvent to 80-100 parts by weight of the acrylic adhesive, continuing to stir at a speed greater than 600 rpm / min for 10-20 min, adding 2-3 parts by weight of a curing agent under continuous stirring, continuing to stir for 20-30 min, filtering with 200-300 mesh gauze, discarding the filter residue, and then standing for 0.5-2 hours to defoam, to obtain the low-temperature foaming heat-reducing viscosity-reducing glue.
10. A low-temperature foaming heat-reducing adhesive film, characterized in that: It is prepared by the following method: The low-temperature foaming heat-reducing adhesive as described in any one of claims 1 to 8 is evenly coated on the substrate, the dry adhesive thickness is controlled to be 50-60 μm, baked at 70-80° C. for 3-5 minutes, cooled to room temperature, and then covered with a release film on the adhesive surface, and then aged at 50-60° C. for 2-4 days to obtain the low-temperature foaming heat-reducing adhesive film.
Citation Information
Patent Citations
Protective film with heating-reducible adhesion and preparation method thereof
CN106433506A
Reactive thermal visbreaking acrylate adhesive, protective film and application of reactive thermal visbreaking acrylate adhesive and protective film
CN115926691A
Adhesive and preparation method thereof, and adhesive layer and heat-reducing adhesive tape prepared from adhesive
CN110938394A
Low-temperature thermal visbreaking adhesive tape and preparation method thereof
CN111647365A