Electrolyte-resistant pressure-sensitive adhesive for new energy battery cell, preparation method of electrolyte-resistant pressure-sensitive adhesive, adhesive tape and test method of adhesive tape
By introducing modified functional monomers such as 4-tert-butyl cup [6] aromatic hydrocarbons into the electrolyte-resistant hydraulic pressure-sensitive adhesive, the problem of existing tape reacting with electrolyte in lithium-ion batteries was solved, and high-stability tape was prepared. Its performance is evaluated through assembly testing methods, achieving excellent application in new energy battery cells.
Patent Information
- Application Number
- CN202411184457.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing electrolyte-resistant acrylic pressure-sensitive adhesives are prone to react with electrolytes in high-energy-density lithium-ion batteries, resulting in discoloration, contamination and degradation of performance. The existing testing methods cannot accurately evaluate their electrochemical stability in actual applications.
Using electrolytic hydraulic pressure-sensitive adhesives including soft monomers, hard monomers, modified functional monomers 4-tert-butyl cups [6] aromatic hydrocarbons, etc., to prepare high chemical stability through specific reaction steps and combinations of additives. and high thermal stability tape and test its electrochemical stability by assembling button half-cell.
It provides electrolytic hydraulic pressure-sensitive tape with excellent bonding properties and stability in high temperature and chemical environments. It can accurately evaluate its electrochemical stability through redox curve testing, and is suitable for the application of new energy battery cells.
Smart Images

Figure CN119081598A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a field, and in particular to an electrolyte-resistant pressure-sensitive adhesive for new energy batteries, a preparation method thereof, an adhesive tape, and a testing method for the adhesive tape. Background Art
[0002] With the rapid rise of basic industries such as energy, transportation, and communications, the lithium-ion battery industry is facing greater challenges after experiencing rapid growth. As a raw material for the battery industry, adhesives are used in small quantities, but they have a very large impact on the performance and product quality of batteries. With the rapid development of the new energy industry, the pressure-sensitive adhesives used in power lithium batteries, as one of the key materials in battery manufacturing, are especially important for the fixation of electrodes and diaphragms, battery packaging, and other links. Based on safety, electrochemical stability, and other considerations, pressure-sensitive adhesives with excellent thermal stability and electrochemical stability are more suitable for lithium-ion batteries. Therefore, the development of pressure-sensitive adhesives that are resistant to high temperatures, solvents, and have high electrochemical stability is very necessary and challenging.
[0003] The solvent resistance of acrylic pressure-sensitive adhesives is mainly determined by the rigid structure of the molecular chain and special functional groups. At present, electrolyte-resistant acrylic tapes will come into contact with the strong polar electrolyte in lithium-ion batteries during the application of high-energy-density lithium-ion batteries. Conventional acrylic tapes are prone to discoloration, yellowing, blackening and carbonization, which not only pollutes the electrolyte, but also seriously affects the performance and safety of lithium-ion batteries. At present, most acrylic tape products improve chemical stability and electrolyte resistance by adjusting the molecular chain structure and doping with special functional groups, such as providing hydrophobic long-chain alkyl (-CH2-) and fluorinated groups (-CF3), and providing chemically stable strong CC bonds, CO bonds or CN bonds. However, it is not clear whether there is an electrochemical reaction with the electrolyte components, thereby affecting the overall performance of lithium-ion batteries.
[0004] Existing electrolyte-resistant acrylic pressure-sensitive adhesives only rely on testing the peeling force performance after immersion in electrolyte, or analyzing the mass change after immersion in electrolyte to determine whether there is swelling and dissolution. Most of the electrolyte immersion test environments cannot even reach oxygen and water-free, and the influence of the chemical changes of the electrolyte itself in a conventional air environment is not ruled out. These test methods can only be used as preliminary evaluation methods for the electrolyte resistance of the tape, and cannot clearly indicate whether the tape undergoes electrochemical reactions with the electrolyte components during actual application. The present invention mainly provides an electrolyte-resistant pressure-sensitive tape product with high chemical stability and high thermal stability for new energy batteries, and analyzes its electrochemical stability by assembling button half-cells, which can better adapt to the application and development of lithium-ion batteries. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an electrolyte-resistant pressure-sensitive adhesive for new energy batteries, a preparation method thereof, an adhesive tape and a testing method for the adhesive tape in view of the deficiencies in the above-mentioned prior art.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: In the first aspect of the present invention, an electrolyte-resistant pressure-sensitive adhesive for new energy batteries is provided, comprising the following raw material components in parts by weight:
[0007] 10-30 parts of soft monomer, 5-15 parts of hard monomer, 4-6 parts of modified functional monomer, 1.5-6 parts of other functional monomers, 0.15-0.6 parts of initiator, 1-6 parts of crosslinking monomer, 50-80 parts of organic solvent;
[0008] Wherein, the modified functional monomer is 4-tert-butylcalix[6]arene.
[0009] Preferably, the soft monomer is selected from one or more of ethyl acrylate, butyl acrylate and isooctyl acrylate.
[0010] Preferably, the hard monomer is selected from one or more of methyl methacrylate, styrene and acrylonitrile.
[0011] Preferably, the cross-linking monomer is selected from one or more of acrylic acid and methacrylic acid.
[0012] Preferably, the other functional monomers are selected from one or more of vinyl tris(2-methoxyethoxy)silane, glycidyl methacrylate, and acryloylmorpholine.
[0013] Preferably, the soft monomer is a mixture of isooctyl acrylate and ethyl acrylate, the hard monomer is methyl methacrylate, the crosslinking monomer is methacrylic acid, and the other functional monomer is vinyl tris (2-methoxyethoxy) silane;
[0014] The organic solvent was a mixture of toluene and ethyl acetate.
[0015] The second aspect of the present invention provides a method for preparing the electrolyte-resistant pressure-sensitive adhesive for new energy batteries as described above, comprising the following steps:
[0016] S1. In an inert gas atmosphere, soft monomers, hard monomers, cross-linking monomers, other functional monomers and organic solvents are mixed and stirred evenly, and the first part of the initiator is first added, and the reaction is carried out at 67° C.-70° C. for 1 h-2 h to obtain a first reaction solution;
[0017] S2, adding the second part of the initiator to the first reaction solution, stirring and reacting at 70° C.-72° C. for 1.5 h-3 h to obtain a second reaction solution;
[0018] S3. Add 4-tert-butylcalix[6]arene and the remaining third part of the initiator to the second reaction liquid, stir and react at 75°C-80°C for 3h-6h to obtain an electrolytic pressure-sensitive adhesive with a solid content of 35-40%, a weight average molecular weight of 60w-80w, and a glass transition temperature of -25 to -40°C.
[0019] The third aspect of the present invention provides an electrolyte pressure sensitive adhesive tape for new energy batteries, which is prepared by the following method: the electrolyte pressure sensitive adhesive for new energy batteries as described above is mixed with a curing agent and a pigment, stirred evenly, and then evenly coated on a substrate, the adhesive surface is adhered to a release film, and matured to obtain the electrolyte pressure sensitive adhesive tape for new energy batteries.
[0020] Preferably, the electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries is prepared by the following method: adding GA530 curing agent and inorganic blue pigment to the electrolyte-resistant pressure-sensitive adhesive for new energy batteries, stirring evenly, and evenly coating the obtained mixed glue on aluminum foil, laminating the adhesive surface with a release film, and aging at 50-60° C. for 12-48 hours to obtain the electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries;
[0021] The addition amounts of GA530 curing agent and inorganic blue pigment are 0.5-2% and 2.5-10% of the total mass of the mixed glue respectively.
[0022] A fourth aspect of the present invention provides a method for testing the electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries as described above, comprising the following steps:
[0023] The electrolyte-resistant pressure-sensitive tape for new energy batteries is used as the positive electrode material and metallic lithium is used as the negative electrode material to assemble into a button half-cell. The redox curve of the button half-cell is then tested, and the electrochemical stability is judged based on the test result of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
[0024] The beneficial effects of the present invention are:
[0025] The present invention provides an electrolyte-resistant pressure-sensitive adhesive, an adhesive tape product and a test method for the adhesive tape product for new energy batteries. The 4-tert-butylcalix[6]arene added to the electrolyte-resistant pressure-sensitive adhesive of the present invention is a macrocyclic compound, which is composed of six benzene rings connected together by a shared carbon atom and is also connected to six tert-butyl substituents. Its excellent ring structure makes the structure have high thermal stability, that is, it can maintain stability at a relatively high temperature, which makes it have good durability when used in a high temperature environment. In addition, the 4-tert-butylcalix[6]arene also exhibits good chemical stability and is not easy to react with substances such as acids and alkalis, which increases its safety and reliability in use. The electrolyte-resistant pressure-sensitive adhesive prepared by the present invention by adding 4-tert-butylcalix[6]arene not only has excellent bonding properties in a high temperature environment, but also has good stability in a chemical environment, and is very suitable for use as a pressure-sensitive adhesive for new energy batteries.
[0026] In the testing method provided by the present invention, the redox curve is tested after the tape is produced and assembled into a button battery, and the electrochemical stability is judged according to the test result of the redox curve, so as to evaluate the performance of the electrolyte-resistant pressure-sensitive tape, and the evaluation result can reflect the performance of the tape in actual application. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Redox curves of the batteries assembled in Test Examples 1 to 3. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0029] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0030] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0031] The present invention provides an electrolyte-resistant pressure-sensitive adhesive for new energy batteries, comprising the following raw material components in parts by weight:
[0032] 10-30 parts of soft monomer, 5-15 parts of hard monomer, 4-6 parts of modified functional monomer, 1.5-6 parts of other functional monomers, 0.15-0.6 parts of initiator, 1-6 parts of crosslinking monomer, 50-80 parts of organic solvent;
[0033] Wherein, the modified functional monomer is 4-tert-butylcalix[6]arene.
[0034] In a preferred embodiment, the soft monomer is selected from one or more of ethyl acrylate, butyl acrylate, and isooctyl acrylate.
[0035] In a preferred embodiment, the hard monomer is selected from one or more of methyl methacrylate, styrene, and acrylonitrile.
[0036] In a preferred embodiment, the cross-linking monomer is selected from one or more of acrylic acid and methacrylic acid.
[0037] In a preferred embodiment, the other functional monomers are selected from one or more of vinyl tris(2-methoxyethoxy)silane, glycidyl methacrylate, and acryloylmorpholine.
[0038] In a preferred embodiment, the soft monomer is a mixture of isooctyl acrylate and ethyl acrylate, the hard monomer is methyl methacrylate, the crosslinking monomer is methacrylic acid, and the other functional monomer is vinyl tris(2-methoxyethoxy)silane.
[0039] In a preferred embodiment, the organic solvent is a mixture of toluene and ethyl acetate.
[0040] The present invention also provides a method for preparing the above electrolyte-resistant pressure-sensitive adhesive for new energy batteries, comprising the following steps:
[0041] S1. In an inert gas atmosphere, soft monomers, hard monomers, cross-linking monomers, other functional monomers and organic solvents are mixed and stirred evenly, and the first part of the initiator is first added, and the reaction is carried out at 67° C.-70° C. for 1 h-2 h to obtain a first reaction solution;
[0042] S2, adding the second part of the initiator to the first reaction solution, stirring and reacting at 70° C.-72° C. for 1.5 h-3 h to obtain a second reaction solution;
[0043] S3. Add 4-tert-butylcalix[6]arene and the remaining third part of the initiator to the second reaction liquid, stir and react at 75°C-80°C for 3h-6h to obtain an electrolytic pressure-sensitive adhesive with a solid content of 35-40%, a weight average molecular weight of 60w-80w, and a glass transition temperature of -25 to -40°C.
[0044] 4-tert-butylcalix[6]arene is a macrocyclic compound consisting of six benzene rings connected together by shared carbon atoms and six tert-butyl substituents. Its excellent ring structure makes the structure have high thermal stability, that is, it can maintain stability at higher temperatures, which makes it have good durability when used in high temperature environments. In addition, it also exhibits good chemical stability and is not easy to react with acids, alkalis and other substances, which increases its safety and reliability in use. Therefore, the electrolyte-resistant pressure-sensitive adhesive prepared by the present invention not only has excellent bonding properties in high temperature environments, but also has good stability in chemical environments.
[0045] The present invention also provides an electrolyte pressure sensitive adhesive tape for new energy batteries, which is prepared by the following method: mixing the above electrolyte pressure sensitive adhesive for new energy batteries with a curing agent and a pigment, stirring evenly, and then evenly coating it on a substrate, laminating the adhesive surface with a release film, and aging to obtain the electrolyte pressure sensitive adhesive tape for new energy batteries.
[0046] In a preferred embodiment, the electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries is prepared by the following method: adding GA530 curing agent and inorganic blue pigment to the electrolyte-resistant pressure-sensitive adhesive for new energy batteries, stirring evenly, and evenly coating the obtained mixed glue on the aluminum foil, laminating the adhesive surface with a release film, and aging at 50-60° C. for 12-48 hours to obtain the electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries;
[0047] The addition amounts of GA530 curing agent and inorganic blue pigment are 0.5-2% and 2.5-10% of the total mass of the mixed glue respectively.
[0048] The present invention also provides a method for testing the above electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries, comprising the following steps:
[0049] The electrolyte-resistant pressure-sensitive tape for new energy batteries is used as the positive electrode material, and metallic lithium is used as the negative electrode material to be assembled into a button half-cell. The redox curve of the button half-cell is then tested, and the electrochemical stability is judged based on the test results of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
[0050] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0051] Source of raw materials:
[0052] Isooctyl acrylate, ethyl acrylate, methyl methacrylate, and methacrylic acid were purchased from Shanghai Hechuang Chemical Co., Ltd.; 4-tert-butylcalix[6]arene was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; vinyltri(2-methoxyethoxy)silane was purchased from Nanjing Youpu Chemical Co., Ltd.; toluene and ethyl acetate were purchased from Qingdao Hefeng Chemical Co., Ltd. of industrial grade; azobisisoheptanenitrile (ABVN) was purchased from Sinopharm Reagent of analytical grade.
[0053] Example 1
[0054] An electrolyte-resistant pressure-sensitive adhesive for new energy batteries, the preparation method of which comprises the following steps:
[0055] The raw materials and their proportions are as follows:
[0056] Soft monomer: 10 parts of isooctyl acrylate, 5 parts of ethyl acrylate; hard monomer: 10 parts of methyl methacrylate; cross-linking monomer: 5 parts of methacrylic acid; modified functional monomer: 5 parts of 4-tert-butylcalix[6]arene; other functional monomers: 4 parts of vinyltri(2-methoxyethoxy)silane; organic solvent: 11 parts of toluene and 50 parts of ethyl acetate; initiator: 0.2 parts of azobisisoheptonitrile.
[0057] S1. In an inert gas atmosphere, according to the following ratio, soft monomers, hard monomers, cross-linking monomers, other functional monomers and organic solvents are mixed and stirred evenly, and the first part of the initiator (specifically 1 / 4 of the total mass of azobisisoheptanenitrile) is first added, and the reaction is carried out at 68° C. for 2 h to obtain a first reaction solution;
[0058] S2, adding the second part of the initiator (specifically 1 / 4 of the total mass of azobisisoheptanenitrile) to the first reaction solution, stirring and reacting at 72° C. for 3 h to obtain a second reaction solution;
[0059] S3. Add 4-tert-butylcalix[6]arene and the remaining third part of the initiator (specifically 1 / 2 of the total mass of azobisisoheptanenitrile) to the second reaction liquid, stir and react at 80°C for 5 hours to obtain an electrolytic pressure-sensitive adhesive with a solid content of 38%, a weight-average molecular weight of 70w, and a glass transition temperature of -32°C.
[0060] A liquid-sensitive adhesive tape resistant to electrolyte for new energy batteries is prepared by the following method: adding a GA530 curing agent and an inorganic blue pigment to the liquid-sensitive adhesive resistant to electrolyte for new energy batteries, stirring evenly, and evenly coating the obtained mixed adhesive on a 20-μm aluminum foil, laminating a release film on the adhesive surface, and aging at 55° C. for 24 hours to obtain the liquid-sensitive adhesive tape resistant to electrolyte for new energy batteries;
[0061] The addition amounts of GA530 curing agent and inorganic blue pigment are 1% and 5% of the total mass of the mixed glue, respectively.
[0062] Comparative Example 1
[0063] This example is basically the same as Example 1, except that in the preparation of the electrolytic pressure sensitive adhesive in this example, 4-tert-butylcalix[8]arene is used instead of 4-tert-butylcalix[6]arene in Example 1. The electrolytic pressure sensitive adhesive prepared in this example has a solid content of 36%, a weight average molecular weight of 72w, and a glass transition temperature of -38°C.
[0064] Comparative Example 2
[0065] This example is basically the same as Example 1, except that in the preparation of the electrolytic pressure sensitive adhesive in this example, 4-tert-butylcalix[4]arene is used instead of 4-tert-butylcalix[6]arene in Example 1. The electrolytic pressure sensitive adhesive prepared in this example has a solid content of 35%, a weight average molecular weight of 68w, and a glass transition temperature of -30°C.
[0066] Comparative Example 3
[0067] This example is basically the same as Example 1, except that 7 parts by weight of 4-tert-butylcalix[6]arene is added in the preparation of the electrolytic pressure sensitive adhesive in this example. The solid content of the electrolytic pressure sensitive adhesive prepared in this example is 37%, the weight average molecular weight is 70w, and the glass transition temperature is -40°C.
[0068] Comparative Example 4
[0069] This example is basically the same as Example 1, except that 3 parts by weight of 4-tert-butylcalix[6]arene is added in the preparation of the electrolytic pressure sensitive adhesive in this example. The solid content of the electrolytic pressure sensitive adhesive prepared in this example is 37%, the weight average molecular weight is 68w, and the glass transition temperature is -28°C.
[0070] Comparative Example 5
[0071] This example is basically the same as Example 1, except that 4-tert-butylcalix[6]arene is not added in the preparation of the electrolytic pressure sensitive adhesive in this example. The solid content of the electrolytic pressure sensitive adhesive prepared in this example is 36.5%, the weight average molecular weight is 65w, and the glass transition temperature is -25°C.
[0072] The following performance tests were performed on the electrolyte-resistant pressure-sensitive adhesive tapes prepared in Example 1 and Comparative Example 5:
[0073] 1. 180° peel strength test standard: Test standard: GB / T 2792-2014 Adhesive tape peel strength test;
[0074] 2. High temperature resistance is determined by the displacement change under high temperature holding force for 72 hours. Holding force test standard: GB / T 4851-2014 Test method for adhesive tape holding force and adhesive tape holding force.
[0075] 3. The test method for electrolyte resistance is:
[0076] The adhesive layer of the tape is attached to an aluminum sheet to prepare a test sample, which is completely immersed in an electrolyte, wherein the electrolyte solute includes 1 mol of LiPF6, and the solvent includes ethylene carbonate: diethyl carbonate: ethyl methyl carbonate = 3:5:2 (volume ratio); soak at 85°C for 8h, cool to room temperature, and then test the 180° peel strength according to the national standard GB / T2792-2014 method.
[0077] The test results are shown in Table 1 below:
[0078] Table 1
[0079]
[0080]
[0081] According to the test results in Table 1, the tape of Example 1 has a high peeling force, and does not fall off or dissolve after being immersed in lithium ion electrolyte at 85° C. for 8 hours, and the viscosity can be maintained at 40%-50%, indicating that it has excellent electrolyte resistance.
[0082] By comparing the results between Example 1 and Comparative Example 5, it can be seen that the modified polyacrylate prepared by adding 4-tert-butylcalix[6]arene has better peeling performance and appearance before and after immersion in electrolyte, and has good high temperature resistance, which will not affect the use of the tape and will not affect the appearance of the electrolyte.
[0083] By comparing the performance data between Example 1 and Comparative Examples 1 and 2, it can be seen that the size of the added calixarene will affect the performance of the product, among which 4-tert-butylcalix[6]arene has the best bonding performance, high temperature resistance and electrolyte resistance. For acrylic tape, the 4-tert-butylcalix[8]arene macrocyclic structure in Comparative Example 1 is too large, which is not conducive to the cohesion of the tape. The 4-tert-butylcalix[4]arene macrocyclic structure in Comparative Example 2 still has room for improvement, so 4-tert-butylcalix[6]arene is selected as the most preferred. By comparing the data between Example 1 and Comparative Examples 3 and 4, it can be seen that the excessive addition of 4-tert-butylcalix[6]arene in Comparative Example 3 will also affect the bonding performance of the tape. The addition of too little additives in Comparative Example 4 will reduce the electrolyte resistance. The above results show that the structure and content of the macrocyclic substance added in the electrolyte-resistant pressure-sensitive adhesive have a significant effect on the adhesive layer bonding strength and electrolyte resistance.
[0084] The following is a redox curve test of the electrolytic pressure sensitive adhesive tapes of Example 1, Comparative Example 1, and Comparative Example 5 after they are assembled into button batteries, so as to further evaluate the performance of the electrolytic pressure sensitive adhesive tapes.
[0085] The test method of the redox curve is as follows: the instrument is Shanghai Chenhua electrochemical workstation, cyclic voltammetry (CV) is selected, the starting potential (2V) and the ending potential (5V) are set, and the scanning rate is 0.001V / s.
[0086] Test Example 1
[0087] The electrolyte-resistant pressure-sensitive tape prepared in Example 1 was used as the positive electrode material, metallic lithium was used as the negative electrode material, the electrolyte was 1 mol of LiPF6, and the solvent used in the electrolyte included ethylene carbonate: diethyl carbonate: ethyl methyl carbonate = 3:5:2 (volume ratio). A C2025 model button battery was assembled in a glove box, and then the redox curve (CV) of the C2025 model button battery was tested. The electrochemical stability was judged based on the test results of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
[0088] Test Example 2
[0089] The electrolyte-resistant pressure-sensitive tape prepared in Comparative Example 1 was used as the positive electrode material, metallic lithium was used as the negative electrode material, the electrolyte was 1 mol of LiPF6, and the solvent used in the electrolyte included ethylene carbonate: diethyl carbonate: ethyl methyl carbonate = 3:5:2 (volume ratio). A C2025 model button battery was assembled in a glove box, and then the redox curve (CV) of the C2025 model button battery was tested. The electrochemical stability was judged based on the test results of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
[0090] Test Example 3
[0091] The electrolyte-resistant pressure-sensitive tape prepared in Comparative Example 5 was used as the positive electrode material, metallic lithium was used as the negative electrode material, the electrolyte was 1 mol of LiPF6, and the solvent used in the electrolyte included ethylene carbonate: diethyl carbonate: ethyl methyl carbonate = 3:5:2 (volume ratio). A C2025 model button battery was assembled in a glove box, and then the redox curve (CV) of the C2025 model button battery was tested. The electrochemical stability was judged based on the test results of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
[0092] The batteries assembled in Test Examples 1 to 3 were subjected to redox curve (CV) tests, and their electrochemical stability was determined by analyzing the redox peaks. The test results are as follows: Figure 1 As shown: (a) is test case 1, (b) is test case 2, and (c) is test case 3. Figure 1 Analysis shows that Test Example 3 has an oxidation peak at a potential of 3.45V and a reduction peak at a potential of 3.93V, indicating that the conventional acrylic tape has poor electrochemical stability and cannot be used in scenarios where it comes into contact with lithium ion electrolytes; the CV curves of Test Example 1 do not show obvious oxidation-reduction peaks, indicating that adding 4-tert-butylcalix[6]arene and 4-tert-butylcalix[8]arene to polyacrylate can achieve higher electrochemical stability; and according to the test results in Table 1, adding 4-tert-butylcalix[6]arene to the electrolyte-resistant pressure-sensitive adhesive can obtain better bonding properties, so it is selected as the present invention.
[0093] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. An electrolyte-resistant pressure-sensitive adhesive for new energy batteries, characterized in that: The invention comprises the following raw material components by weight: 10-30 parts of soft monomer, 5-15 parts of hard monomer, 4-6 parts of modified functional monomer, 1.5-6 parts of other functional monomers, 0.15-0.6 parts of initiator, 1-6 parts of crosslinking monomer, 50-80 parts of organic solvent; Wherein, the modified functional monomer is 4-tert-butylcalix[6]arene.
2. The electrolyte-resistant pressure-sensitive adhesive for new energy batteries according to claim 1, characterized in that: The soft monomer is selected from one or more of ethyl acrylate, butyl acrylate and isooctyl acrylate.
3. The electrolyte-resistant pressure-sensitive adhesive for new energy batteries according to claim 1, characterized in that: The hard monomer is selected from one or more of methyl methacrylate, styrene and acrylonitrile.
4. The electrolyte-resistant pressure-sensitive adhesive for new energy batteries according to claim 1, characterized in that: The cross-linking monomer is selected from one or more of acrylic acid and methacrylic acid.
5. The electrolyte-resistant pressure-sensitive adhesive for new energy batteries according to claim 1, characterized in that: The other functional monomers are selected from one or more of vinyl tris(2-methoxyethoxy)silane, glycidyl methacrylate, and acryloyl morpholine.
6. The electrolyte-resistant pressure-sensitive adhesive for new energy batteries according to claim 1, characterized in that: The soft monomer is a mixture of isooctyl acrylate and ethyl acrylate, the hard monomer is methyl methacrylate, the crosslinking monomer is methacrylic acid, and the other functional monomer is vinyl tris (2-methoxyethoxy) silane; The organic solvent was a mixture of toluene and ethyl acetate.
7. A method for preparing an electrolyte-resistant pressure-sensitive adhesive for new energy batteries as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1. In an inert gas atmosphere, soft monomers, hard monomers, cross-linking monomers, other functional monomers and organic solvents are mixed and stirred evenly, and the first part of the initiator is first added, and the reaction is carried out at 67° C.-70° C. for 1 h-2 h to obtain a first reaction solution; S2, adding the second part of the initiator to the first reaction solution, stirring and reacting at 70° C.-72° C. for 1.5 h-3 h to obtain a second reaction solution; S3. Add 4-tert-butylcalix[6]arene and the remaining third part of the initiator to the second reaction liquid, stir and react at 75°C-80°C for 3h-6h to obtain an electrolytic pressure-sensitive adhesive with a solid content of 35-40%, a weight average molecular weight of 60w-80w, and a glass transition temperature of -25 to -40°C.
8. An electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries, characterized in that: The preparation method is as follows: the electrolyte-resistant pressure-sensitive adhesive for new energy batteries described in any one of claims 1 to 6 is mixed with a curing agent and a pigment, stirred evenly, and then evenly coated on a substrate, the adhesive surface is attached to a release film, and aged to obtain an electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries.
9. The electrolyte-resistant pressure-sensitive adhesive tape for new energy batteries according to claim 8, characterized in that: The preparation method is as follows: adding GA530 curing agent and inorganic blue pigment to the electrolytic pressure sensitive adhesive for new energy batteries, stirring evenly, coating the obtained mixed adhesive evenly on aluminum foil, laminating the adhesive surface with a release film, and aging at 50-60° C. for 12-48 hours to obtain an electrolytic pressure sensitive adhesive tape for new energy batteries; The addition amounts of GA530 curing agent and inorganic blue pigment are 0.5-2% and 2.5-10% of the total mass of the mixed glue respectively.
10. A method for testing an electrolyte-resistant pressure-sensitive adhesive tape for a new energy battery cell as claimed in claim 8 or 9, characterized in that: The following steps are involved: The electrolyte-resistant pressure-sensitive tape for new energy batteries is used as the positive electrode material and metallic lithium is used as the negative electrode material to assemble into a button half-cell. The redox curve of the button half-cell is then tested, and the electrochemical stability is judged based on the test result of the redox curve, thereby evaluating the performance of the electrolyte-resistant pressure-sensitive tape.
Citation Information
Patent Citations
Binder, adhesive tape, preparation method of adhesive tape and electrochemical device
CN115820169A
Water-white-resistant acrylate pressure-sensitive adhesive and preparation method therefor
WO2021197054A1