Macromolecular binder as well as preparation method and application thereof

By using the polymerization products of natural polymers and carbon-carbon double bond compounds under the action of initiators as binders, the bond failure problem caused by volume changes in the charge and discharge process of lithium-ion batteries is solved, which significantly improves the bonding failure problem. Adhesion properties and cycle stability.

CN119081602APending Publication Date: 2024-12-06CHINA ENFI ENG CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411374728.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The volume of the silicon-based negative electrode of lithium-ion batteries changes greatly during charging and discharging, resulting in poor toughness of the adhesive and easy powder removal of active substances.

Method used

The graft copolymerization product of natural polymers and carbon-carbon double bond compounds under the action of initiators is used as the binder. The natural polymers contain hydroxyl groups and/or carboxy groups, and the carbon-carbon double bond compounds contain amino groups and/or carboxy groups. The polymerization reaction forms a polymer binder rich in polar functional groups, enhancing the hydrogen bonding with the silicon-based negative electrode and the current collector, and improving the bonding performance.

Benefits of technology

It significantly improves the bonding performance of the silicon-based negative electrode, reduces the bonding failure and powder peeling of the active material during charging and discharging, and improves the cycle stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068396190000091
    Figure BDA0005068396190000091
Patent Text Reader

Abstract

The invention provides a high-molecular binder as well as a preparation method and application thereof. The polymer binder is a graft copolymerization product of a natural polymer and a carbon-carbon double-bond compound under the action of an initiator, the natural polymer contains hydroxyl and / or carboxyl, and the carbon-carbon double-bond compound contains amino and / or carboxyl. A polymerization product of a natural polymer and a carbon-carbon double bond compound under the action of an initiator is used as the binder, and the binder has rich polar functional groups and can form hydrogen bonds with hydroxyl groups on the surfaces of the silicon-based negative electrode and the current collector, so that the adhesion effect is improved, and the bonding performance of the silicon-based negative electrode and the current collector is remarkably improved; and the bonding failure and pulverization peeling of the active material caused by volume expansion of the silicon-based negative electrode of the lithium ion battery in the charging and discharging process are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a polymer binder, a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in mobile power supplies and energy storage devices due to their high energy, long life and portability. However, with the development of science and technology, the energy density of lithium-ion batteries can no longer meet the growing demand for large-capacity, high-power batteries in electric vehicles, and scientists have been constantly looking for new electrode materials with higher energy and power density. The theoretical upper limit of the energy density of traditional graphite negative electrodes is 372mAh·g -1 , the existing technology has approached the theoretical value and it is difficult to break through further.

[0003] Silicon has a high theoretical specific capacity (4200mAh g -1 ), high safety, environmental friendliness and high abundance, etc., have attracted much attention. However, there are also some key issues to be resolved, such as the huge volume change of silicon-lithium alloy leading to bonding failure and peeling. Traditional polyvinylidene fluoride binder is no longer suitable for silicon-based negative electrode materials due to its weak van der Waals force with silicon-based negative electrode and current collector. Although the currently commercially available sodium hydroxymethyl cellulose and styrene-butadiene rubber work well for graphite negative electrodes, due to their weak viscoelasticity, they have poor bonding effect on high energy density silicon-carbon negative electrodes.

[0004] Patent CN 110970622 A discloses a water-based binder obtained by condensation reaction of a carboxyl-containing polymer and an amino-containing silane coupling agent. CN 109935832 A discloses a lithium-ion battery silicon-based negative electrode binder, comprising 20 to 60 parts of a main binder and 10 to 35 parts of an auxiliary binder, wherein the main binder is sodium alginate, and the auxiliary binder comprises 5 to 20 parts of sodium carboxymethyl cellulose and at least one of styrene-butadiene rubber and 5 to 15 parts of gelatin. CN 109411757 A discloses a binder for lithium-ion battery silicon-based negative electrode, comprising 10%-80% of a linear polymer, 10%-60% of a conductive polymer, and 10-60% of a self-healing polymer. However, the bonding performance of the binder provided by the above scheme still needs to be improved. Summary of the invention

[0005] The main purpose of the present invention is to provide a polymer binder, a preparation method and application thereof, so as to solve the problem in the prior art that the volume of silicon-based negative electrodes changes greatly during charging and discharging, and the binder has poor toughness, resulting in easy pulverization and peeling of active materials.

[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a polymer binder is provided, which is a graft copolymerization product of a natural polymer and a carbon-carbon double bond compound under the action of an initiator, the natural polymer contains hydroxyl and / or carboxyl groups, and the carbon-carbon double bond compound contains amino and / or carboxyl groups.

[0007] Furthermore, the natural polymer includes one or more of sodium alginate, konjac gum, guar gum, peach gum, xanthan gum and gum arabic; and / or the weight average molecular weight of the natural polymer is 100,000 to 2,000,000; and / or the carbon-carbon double bond compound includes one or more of acrylamide, acrylic acid, methacrylic acid, hydroxyethyl methacrylate and dimethylaminopropyl acrylamide; preferably, the weight ratio of the natural polymer to the carbon-carbon double bond compound is 1:(0.1 to 10), more preferably 1:(0.2 to 8).

[0008] Further, the weight ratio of the natural polymer to the initiator is 1:(0.01-0.6); preferably 1:(0.08-0.5); and / or the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

[0009] According to another aspect of the present invention, a method for preparing the above-mentioned polymer binder of the present invention is provided, comprising the following steps: step S1, mixing natural polymers, carbon-carbon double bond compounds and water to obtain a mixed raw material; step S2, under an inert gas atmosphere, adding an initiator aqueous solution to the mixed raw material to carry out a polymerization reaction to obtain a polymer binder.

[0010] Furthermore, the mass concentration of the mixed raw materials is 20 to 160 g / L; and / or the mixing temperature is 40 to 60° C., and the time is 30 to 60 min; preferably, the mixing is carried out under stirring, and the stirring speed is 350 to 450 r·min -1 .

[0011] Furthermore, the weight ratio of the natural polymer to the initiator in the initiator aqueous solution is 1:(0.01-0.6); and / or the dripping speed of the initiator aqueous solution is 1-10 mL / min; and / or the polymerization temperature is 40-60° C., and the time is 1.5-2.5 h; preferably, the preparation method also includes: purifying and freeze-drying the feed liquid after the polymerization reaction in sequence to obtain a polymer binder.

[0012] According to another aspect of the present invention, there is provided a silicon-based negative electrode, comprising a silicon-based active material, a conductive additive and the polymer binder of the present invention.

[0013] Furthermore, the weight ratio of the silicon-based active material, the conductive additive and the binder is (60-98):(1-20):(1-20); and / or the silicon-based active material includes one or more of nano-silicon material, silicon oxide material, silicon-carbon composite material and silicon oxide-carbon composite material.

[0014] According to another aspect of the present invention, a method for preparing the silicon-based negative electrode of the present invention is provided, wherein a silicon-based active material, a conductive additive and the polymer binder of the present invention are mixed with water to obtain a slurry; the slurry is coated on the surface of the current collector, and then air drying and vacuum drying are performed in sequence, the air drying temperature is 40 to 60°C, the time is 1.5 to 2.5 hours, and the vacuum drying temperature is 90 to 110°C, the time is 10 to 14 hours, to obtain a silicon-based negative electrode.

[0015] According to another aspect of the present invention, a lithium-ion battery is provided, comprising the silicon-based negative electrode of the present invention.

[0016] By applying the technical solution of the present invention, the polymerization product of natural polymers and carbon-carbon double bond compounds under the action of an initiator is used as a binder. The binder has rich polar functional groups and can form hydrogen bonds with the hydroxyl groups on the surface of the silicon-based negative electrode and the current collector, thereby increasing the adhesion effect, significantly improving the bonding performance of the silicon-based negative electrode and the current collector, and reducing the bonding failure and powdering and peeling of the active material caused by the volume expansion of the silicon-based negative electrode of the lithium-ion battery during the charging and discharging process. DETAILED DESCRIPTION

[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0018] As described in the background of the present invention, the prior art has the problem that the volume of the silicon-based negative electrode changes greatly during the charge and discharge process, and the binder has poor toughness, which leads to easy pulverization and peeling of the active material. In order to solve the above problems, in a typical embodiment of the present invention, a polymer binder is provided, which is a graft copolymerization product of a natural polymer and a carbon-carbon double bond compound under the action of an initiator, the natural polymer contains hydroxyl and / or carboxyl groups, and the carbon-carbon double bond compound contains amino and / or carboxyl groups.

[0019] In view of the huge volume expansion of the silicon-based negative electrode of the lithium-ion battery during the charge and discharge process, which leads to the problems of active material bonding failure and powdering and peeling, the present invention provides a new solution: the polymerization product of natural polymers and carbon-carbon double bond compounds under the action of an initiator is used as a binder. The natural polymer is rich in functional groups such as hydroxyl and carboxyl groups, but has poor toughness, and it is difficult to completely solve the bonding failure caused by the poor toughness of the binder. The carbon-carbon double bonds in the carbon-carbon double bond compounds rich in functional groups such as amino and carboxyl groups can be opened into single bonds under the action of an initiator, which is convenient for grafting onto the natural polymer skeleton. Therefore, the problem of poor toughness of the natural polymer can be significantly improved. At the same time, the surface of the polymerization product of the natural polymer and the carbon-carbon double bond compound under the action of an initiator still has more polar functional groups. These polar groups can form hydrogen bonds with the hydroxyl groups on the surface of the silicon-based negative electrode and the current collector (such as copper), increase the adhesion between the three, solve the bonding failure problem of the silicon-based negative electrode during the charge and discharge process, improve the cycle stability of the lithium-ion battery, and provide an effective way to obtain high-performance lithium-ion batteries.

[0020] In a preferred embodiment, the natural polymer includes one or more of sodium alginate, konjac gum, guar gum, peach gum, xanthan gum and gum arabic; and / or the weight average molecular weight of the natural polymer is 100,000 to 2,000,000; and / or the carbon-carbon double bond compounds include one or more of acrylamide, acrylic acid, methacrylic acid, hydroxyethyl methacrylate and dimethylaminopropyl acrylamide. The natural polymers with the above molecular weights have appropriate viscosity and are rich in polar functional groups such as hydroxyl and carboxyl groups, which are more conducive to the formation of hydrogen bonds during the bonding process, and further have the characteristics of being environmentally friendly and low cost.

[0021] Preferably, the weight ratio of natural polymers to carbon-carbon double bond compounds is 1:(0.1-10), more preferably 1:(0.2-8). The structural complementarity between natural polymers and carbon-carbon double bond compounds can be utilized to make the formed polymer product have richer polar functional groups and higher toughness, thereby forming a more stable and powerful electrochemical connection with the silicon active particles through hydrogen bonding, increasing the adhesion, solving the problem of bonding failure of the silicon-based negative electrode during the charge and discharge process, and further improving the cycle stability of the lithium-ion battery.

[0022] In order to make the type and addition amount of the initiator more suitable for the polymerization system of the present invention, so that the prepared polymer adhesive can have more abundant polar groups while efficiently initiating polymerization, thereby further improving the bonding performance, in a preferred embodiment, the weight ratio of the natural polymer to the initiator is 1:(0.01-0.6); preferably 1:(0.08-0.5); and / or the initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

[0023] In another typical embodiment of the present invention, a method for preparing the above-mentioned polymer binder of the present invention is also provided, comprising the following steps: step S1, mixing natural polymers, carbon-carbon double bond compounds and water to obtain a mixed raw material; step S2, under an inert gas atmosphere, adding an initiator aqueous solution to the mixed raw material to carry out a polymerization reaction to obtain a polymer binder.

[0024] The present invention first mixes natural polymers, carbon-carbon double bond compounds with water, then drips an initiator aqueous solution under an inert gas atmosphere to perform a polymerization reaction, during which the carbon-carbon double bonds are opened to become single bonds, which are respectively grafted onto the natural polymer skeleton to form a three-dimensional network binder. The above preparation method is simple, easy to operate, and has little environmental pollution. The prepared polymer binder has good adhesion and can significantly reduce the adhesion failure of the silicon-based negative electrode. Even if the silicon-based negative electrode has a large volume change during the charge and discharge process, the binder has sufficient toughness to prevent the active material from being powdered and peeled off.

[0025] In order to further improve the mixing uniformity of the raw materials, thereby providing a more suitable liquid environment for the polymerization reaction, in a preferred embodiment, the mass concentration of the mixed raw materials is 20-160 g / L; and / or the mixing temperature is 40-60° C., and the time is 30-60 min; preferably, the mixing is carried out under stirring, and the stirring speed is 350-450 r·min -1 .

[0026] In order to further increase the polymerization reaction rate and improve the polar group richness of the polymerization product, in a preferred embodiment, the weight ratio of the natural polymer to the initiator in the initiator aqueous solution is 1: (0.01-0.6); and / or the dripping speed of the initiator aqueous solution is 1-10 mL / min; and / or the polymerization temperature is 40-60°C and the time is 1.5-2.5 h; preferably, the preparation method also includes: purifying and freeze-drying the feed solution after the polymerization reaction in sequence to obtain a polymer binder, so that the battery slurry can be directly prepared. The purification method includes extraction and dialysis.

[0027] In another typical embodiment of the present invention, a silicon-based negative electrode is provided, comprising a silicon-based active material, a conductive additive and the above-mentioned polymer binder of the present invention, which has significantly reduced bonding failure phenomenon and significantly improved cycle stability.

[0028] The silicon-based negative electrode can be prepared according to conventional proportions. In a preferred embodiment, the weight ratio of the silicon-based active material, the conductive additive and the binder is (60-98): (1-20): (1-20); and / or the silicon-based active material includes one or more of nano-silicon material, silicon oxide material, silicon-carbon composite material and silicon oxide-carbon composite material. The polymer binder with polar groups on the surface and good toughness of the present invention is more suitable for hydrogen bonding with the hydroxyl groups on the surface of the above active material, and the bonding effect is more significantly improved. The conductive additive can use conventional types in the field, such as one or more of conductive carbon black, SuperP, Ketjen black and conductive graphite, all of which can achieve good matching effects.

[0029] In another typical embodiment of the present invention, a method for preparing the silicon-based negative electrode of the present invention is also provided, wherein the silicon-based active material, the conductive additive and the polymer binder of the present invention are mixed with water to obtain a slurry; the slurry is coated on the surface of the current collector, and then air drying and vacuum drying are performed in sequence, the air drying temperature is 40 to 60° C., the time is 1.5 to 2.5 hours, and the vacuum drying temperature is 90 to 110° C., and the time is 10 to 14 hours, to obtain a silicon-based negative electrode. The current collector includes copper foil and / or aluminum foil.

[0030] In another typical embodiment of the present invention, a lithium-ion battery is provided, comprising the silicon-based negative electrode of the present invention, which has significantly improved cycle stability.

[0031] Typically but not limiting, the weight ratio of natural polymer to carbon-carbon double bond compound is 1:0.1, 1:0.2, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10 or a range consisting of any two of them.

[0032] Typically but not limiting, the weight ratio of natural polymer to initiator is 1:0.01, 1:0.05, 1:0.08, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6 or a range consisting of any two of them.

[0033] Typically but not limiting, the dripping speed of the initiator aqueous solution is 1 mL / min, 2 mL / min, 3 mL / min, 4 mL / min, 5 mL / min, 6 mL / min, 7 mL / min, 8 mL / min, 9 mL / min, 10 mL / min or a range consisting of any two of them.

[0034] Typically but not limiting, the polymerization temperature is 40°C, 45°C, 50°C, 55°C, 60°C, and the polymerization time is 1.5h, 1.8h, 2.0h, 2.2h, 2.5h or a range consisting of any two of them.

[0035] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0036] Example 1

[0037] Preparation of polymer binder:

[0038] Weigh 1.0 g of sodium alginate (weight average molecular weight of 1 million) and 8.0 g of acrylic acid powder respectively, disperse them in a three-necked round-bottom flask filled with 100 mL of deionized water, place the flask in a constant temperature water bath, set the water bath temperature to 50 °C, mix for 30 min, and perform mechanical stirring at a stirring speed of 400 r / min. -1 .

[0039] Then weigh 0.5g of ammonium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 5mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 50°C for 2h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named A).

[0040] Preparation of silicon-based negative electrode:

[0041] Using deionized water as solvent, silicon / carbon composite material, conductive agent Super P and binder A are mixed in a mass ratio of 8:1:1, and then the slurry is evenly coated on copper foil. The copper foil is then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil is transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0042] Example 2

[0043] Preparation of polymer binder:

[0044] 1.0 g of konjac gum (weight average molecular weight of 1 million) and 5.0 g of acrylamide powder were weighed separately and dispersed in a three-necked round-bottom flask filled with 80 mL of deionized water. The flask was placed in a constant temperature water bath with the water bath temperature set to 50 ° C. The mixing time was 30 min and mechanical stirring was performed at a stirring speed of 400 r min. -1 .

[0045] Then weigh 0.4g of potassium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel. Place the constant pressure funnel on a round-bottom flask and pass nitrogen into the round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel and drip the potassium persulfate solution into the flask at a rate of 5mL / min. The entire reaction is carried out under nitrogen. After the reaction is continued at 50°C for 2h, stop heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named B).

[0046] Preparation of silicon-based negative electrode:

[0047] Using deionized water as solvent, silicon / carbon composite material, Super P and binder B are mixed in a mass ratio of 8:1:1, and then the slurry is evenly coated on the copper foil. The copper foil is then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil is transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0048] Example 3

[0049] Preparation of polymer binder:

[0050] 5.0 g peach gum (weight average molecular weight of 1 million) and 1.0 g acrylic acid powder were weighed and dispersed into a three-necked round-bottom flask filled with 80 mL of deionized water. The flask was placed in a constant temperature water bath with the water bath temperature set to 50 °C and the mixing time set to 30 min. Mechanical stirring was performed with the stirring speed set to 400 r min. -1 .

[0051] Then weigh 0.4g of ammonium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel. Place the constant pressure funnel on a round-bottom flask and pass nitrogen into the round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel and drop the ammonium persulfate solution into the flask at a rate of 5mL / min. The entire reaction is carried out under nitrogen. After the reaction is continued at 50°C for 2h, stop heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named C).

[0052] Preparation of silicon-based negative electrode:

[0053] Using deionized water as solvent, nano-silicon material, conductive agent Super P and binder C were mixed in a mass ratio of 9:0.5:0.5, and then the slurry was evenly coated on the copper foil. The copper foil was then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil was transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0054] Example 4

[0055] Preparation of polymer binder:

[0056] 5.0 g of xanthan gum (weight average molecular weight of 1 million) and 3.0 g of methacrylic acid were weighed and dispersed in a three-necked round-bottom flask filled with 100 mL of deionized water. The flask was placed in a constant temperature water bath with the water bath temperature set to 50 °C and the mixing time set to 30 min. Mechanical stirring was performed with the stirring speed set to 400 r·min. -1 .

[0057] Then weigh 0.5g of ammonium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 5mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 50°C for 2h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named D).

[0058] Preparation of silicon-based negative electrode:

[0059] Using deionized water as solvent, silicon dioxide / carbon composite material, conductive agent Super P and binder D are slurried in a mass ratio of 8:1:1, and then the slurry is evenly coated on copper foil. The copper foil is then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil is transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0060] Example 5

[0061] Preparation of polymer binder:

[0062] Weigh 5.0 g of sodium alginate (weight average molecular weight of 100,000) and 0.5 g of acrylic acid powder respectively, disperse them in a three-necked round-bottom flask filled with 100 mL of deionized water, place the flask in a constant temperature water bath, set the water bath temperature to 50 °C, mix for 30 min, and perform mechanical stirring at a stirring speed of 400 r·min -1 .

[0063] Then weigh 0.05g of ammonium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 5mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 50°C for 2h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named E).

[0064] Preparation of silicon-based negative electrode:

[0065] Using deionized water as solvent, silicon / carbon composite material, conductive agent Super P and binder E are mixed in a mass ratio of 8:1:1, and then the slurry is evenly coated on copper foil. The copper foil is then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil is transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0066] Example 6

[0067] Preparation of polymer binder:

[0068] 1.0 g of sodium alginate (weight average molecular weight of 2 million) and 10.0 g of acrylic acid powder were weighed and dispersed in a three-necked round-bottom flask filled with 100 mL of deionized water. The flask was placed in a constant temperature water bath with the water bath temperature set to 50 °C and the mixing time set to 30 min. Mechanical stirring was performed with the stirring speed set to 400 r·min. -1 .

[0069] Then weigh 0.6g of sodium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 5mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 50°C for 2h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named F).

[0070] Preparation of silicon-based negative electrode:

[0071] Using deionized water as solvent, silicon / carbon composite material, conductive agent Super P and binder F were mixed in a mass ratio of 8:1:1, and then the slurry was evenly coated on copper foil. The copper foil was then transferred to a forced air drying oven and dried at 50°C for 2 hours. After drying, the copper foil was transferred to a vacuum drying oven and dried at 100°C for 12 hours to obtain a silicon-based negative electrode.

[0072] Example 7

[0073] Preparation of polymer binder:

[0074] Weigh 1.0 g of sodium alginate (weight average molecular weight of 1 million) and 8.0 g of acrylic acid powder respectively, disperse them in a three-necked round-bottom flask filled with 100 mL of deionized water, place the flask in a constant temperature water bath, set the water bath temperature to 40 °C, mix for 60 min, and perform mechanical stirring at a stirring speed of 350 r·min. -1 .

[0075] Then weigh 0.5g of ammonium persulfate powder, dissolve it in 10mL of deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 1mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 40°C for 2.5h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named G).

[0076] Preparation of silicon-based negative electrode:

[0077] Using deionized water as solvent, silicon / carbon composite material, conductive agent Super P and binder G are mixed in a mass ratio of 6:2:2, and then the slurry is evenly coated on copper foil. The copper foil is then transferred to a forced air drying oven and dried at 40°C for 2.5 hours. After drying, the copper foil is transferred to a vacuum drying oven and dried at 90°C for 14 hours to obtain a silicon-based negative electrode.

[0078] Example 8

[0079] Preparation of polymer binder:

[0080] Weigh 1.0 g of sodium alginate (weight average molecular weight of 1 million) and 8.0 g of acrylic acid powder respectively, disperse them in a three-necked round-bottom flask filled with 100 mL of deionized water, place the flask in a constant temperature water bath, set the water bath temperature to 60 ° C, mix for 30 min, and perform mechanical stirring at a stirring speed of 450 r·min -1 .

[0081] Then weigh 0.5g of ammonium persulfate powder, dissolve it in 10mL deionized water, and move it to a constant pressure funnel, place the constant pressure funnel on a three-mouth round-bottom flask, and pass nitrogen into the three-mouth round-bottom flask to exhaust the air in the flask and the mixed solution. After ventilation for half an hour, open the stopcock of the constant pressure funnel, and drip the ammonium persulfate solution into the flask at a rate of 10mL / min, and keep the nitrogen atmosphere throughout the reaction process. After continuous reaction at 60°C for 1.5h, turn off the heating and stop ventilation. The obtained mixed solution is then purified and freeze-dried to obtain a binder powder (named H).

[0082] Preparation of silicon-based negative electrode:

[0083] Using deionized water as solvent, silicon / carbon composite material, conductive agent Super P and binder H were mixed in a mass ratio of 91:3:6, and then the slurry was evenly coated on copper foil. The copper foil was then transferred to a forced air drying oven and dried at 60°C for 1.5 hours. After drying, the copper foil was transferred to a vacuum drying oven and dried at 110°C for 10 hours to obtain a silicon-based negative electrode.

[0084] Comparative Example 1

[0085] A silicon-based negative electrode was prepared using the method of Example 1 using PVDF binder.

[0086] Comparative Example 2

[0087] 2g of methacrylic anhydride and 15g of alginic acid were dissolved in 100g of water, stirred and dissolved in a glass reactor, cooled to 3°C, and high-purity nitrogen was introduced to exclude oxygen until the oxygen content was less than 3ppm, and the pH value of the mixture solution was adjusted to 7.5-8.5 with 1mol / L NaOH solution, stirred and reacted for 24h, and the product was placed in a dialysis bag, dialyzed for 3 days (the number of water changes was greater than 8 times), and then freeze-dried to obtain the product methacrylic anhydride modified alginic acid. 12g of 2-acrylamide-2-methylpropanesulfonic acid, 6g of methacrylic acid, 15g of methacrylic anhydride modified alginic acid and 0.5g of ammonium persulfate were dissolved in 100g of water, stirred and dissolved in a glass reactor, heated to 65°C, and high-purity nitrogen was introduced to exclude oxygen for 20min, and then reacted for 6h, 0.5g of ammonium persulfate was added to continue the reaction for 6h, and then freeze-dried to obtain a poly (methacrylic acid-co-2-acrylamide-2-methylpropanesulfonic acid) modified alginic acid binder. A silicon-based negative electrode was prepared according to the method of Example 1.

[0088] The silicon-based negative electrode prepared in the above-mentioned embodiment and comparative example was used as the negative electrode, and the metal lithium sheet was used as the counter electrode to assemble button-type batteries, and a 100-cycle test was performed. The results are shown in Table 1.

[0089] Test method:

[0090] 100-cycle capacity retention rate: record the battery's first cycle charging capacity as m0, and the battery's charging capacity at the 100th cycle is m1. At this time, the battery's capacity retention rate at the 100th cycle = 100% × m1 ÷ m0.

[0091] Average peeling force of the electrode: (1) Cut the vacuum-dried electrode into a rectangle of 6 cm long and 2 cm wide, and measure the average thickness of the electrode with a spiral micrometer and record it; (2) Use a double-sided tape of 6 cm long and 2 cm wide to stick the electrode tightly on the glass sheet, with the front of the electrode facing outward; (3) Then stick a 1.8 cm wide transparent tape on the electrode and gently scrape it twice with your hands; (4) Clamp the glass sheet on the upper end of the testing machine mold, and let the transparent tape hang naturally and clamp it on the lower end of the mold; (5) Set the test speed to 10-15 mm·min -1 , input the electrode width and thickness, reset the test machine force to zero, and press the start button; (6) When the test displacement is about 5 cm, press the pause button, save the Excel data, obtain the average peeling force of the electrode, and observe the electrode surface morphology.

[0092] Table 1

[0093]

[0094] As can be seen from the above, compared with the comparative example, the embodiments of the present invention use the polymerization product of natural polymer and carbon-carbon double bond compounds under the action of initiator as a binder, which has rich polar functional groups and can form hydrogen bonds with the hydroxyl groups on the surface of the silicon-based negative electrode and the current collector, thereby increasing the adhesion effect, significantly improving the bonding performance of the silicon-based negative electrode and the current collector, and reducing the active material bonding failure and powdering and peeling caused by the volume expansion of the silicon-based negative electrode of the lithium-ion battery during the charging and discharging process. In addition, it can be seen that when all process parameters are within the preferred range of the present invention, the comprehensive performance of the material is better.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polymer binder, It is characterized in that The polymer binder is a graft copolymerization product of a natural polymer and a carbon-carbon double bond compound under the action of an initiator. The natural polymer contains hydroxyl and / or carboxyl groups, and the carbon-carbon double bond compound contains amino and / or carboxyl groups.

2. The polymer binder according to claim 1, It is characterized in that The natural polymer comprises one or more of sodium alginate, konjac gum, guar gum, peach gum, xanthan gum and gum arabic; and / or The weight average molecular weight of the natural polymer is 100,000 to 2,000,000; and / or The carbon-carbon double bond compound includes one or more of acrylamide, acrylic acid, methacrylic acid, hydroxyethyl methacrylate and dimethylaminopropyl acrylamide; Preferably, the weight ratio of the natural polymer to the carbon-carbon double bond compound is 1:(0.1-10), more preferably 1:(0.2-8).

3. The polymer binder according to claim 1 or 2, It is characterized in that The weight ratio of the natural polymer to the initiator is 1:(0.01-0.6); preferably 1:(0.08-0.5); and / or The initiator includes one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

4. A method for preparing a polymer binder according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step S1, mixing natural polymers, carbon-carbon double bond compounds and water to obtain a mixed raw material; Step S2, under an inert gas atmosphere, dripping an initiator aqueous solution into the mixed raw material to carry out a polymerization reaction to obtain the polymer binder.

5. The preparation method according to claim 4, It is characterized in that The mass concentration of the mixed raw material is 20 to 160 g / L; and / or The mixing temperature is 40-60°C and the time is 30-60 min; preferably, the mixing is carried out under stirring at a stirring speed of 350-450 r·min -1 .

6. The preparation method according to claim 4 or 5, It is characterized in that The weight ratio of the natural polymer to the initiator in the initiator aqueous solution is 1:(0.01-0.6); and / or the dripping speed of the initiator aqueous solution is 1-10 mL / min; and / or The polymerization reaction temperature is 40-60° C., and the reaction time is 1.5-2.5 h. Preferably, the preparation method further comprises: purifying and freeze-drying the feed solution after the polymerization reaction in sequence to obtain the polymer binder.

7. A silicon-based negative electrode, It is characterized in that The invention comprises a silicon-based active material, a conductive additive and the polymer binder according to any one of claims 1 to 3.

8. The silicon-based negative electrode according to claim 7, It is characterized in that The weight ratio of the silicon-based active material, the conductive additive and the binder is (60-98):(1-20):(1-20); and / or The silicon-based active material includes one or more of nano-silicon material, silicon oxide material, silicon-carbon composite material and silicon oxide-carbon composite material.

9. The method for preparing the silicon-based negative electrode according to claim 7 or 8, It is characterized in that Mix a silicon-based active material, a conductive additive, and a polymer binder as described in any one of claims 1 to 3 with water to obtain a slurry; apply the slurry on the surface of a current collector, and then perform air drying and vacuum drying in sequence, wherein the air drying temperature is 40 to 60°C and the time is 1.5 to 2.5 hours, and the vacuum drying temperature is 90 to 110°C and the time is 10 to 14 hours, to obtain the silicon-based negative electrode.

10. A lithium ion battery, It is characterized in that Comprising the silicon-based negative electrode as described in claim 7 or 8.

Citation Information

Patent Citations

  • Binder for lithium ion battery silicon-based anode and preparation method and application of the binder

    CN109411757A

  • Silicon-based negative electrode binder for lithium ion batteries and preparation method of negative electrode sheet using binder

    CN109935832A

  • Water-based adhesive as well as preparation method and application thereof

    CN110970622A