Preparation method of graphene reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials

By using graphene-strengthening resin-based stacked high-temperature adhesive in carbon/carbon composite materials, combining bionic nacre structure and in-situ growth carbon nanotubes, the low bond strength and poor thermal resistance in carbon/carbon material connections are solved. The problem of high bonding strength and good thermal cycle resistance of high-temperature glue is achieved.

CN119081608APending Publication Date: 2024-12-06TIANJIN THERMAL DEFENSE CRAFTSMAN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206251.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing bonding technology is used in the aerospace field for the connection of carbon/carbon composite materials, which has problems such as low bonding strength, poor thermal shock resistance, and limited high-temperature usage effects, and is particularly difficult to prepare large components with complex structures.

Method used

Graphene-strengthening resin-based stacked high-temperature adhesive is used to grow carbon nanotubes in situ in the graphene sheet layer, and combine the bionic nacre structure to improve the high temperature and thermal cycle resistance of the adhesive.

Benefits of technology

The high bonding strength and good thermal cycle resistance of high-temperature glue are achieved. The bonding strength reaches 10.74MPa at 250℃, and the bonding strength is provided in the range of 800 to 1300℃, and the strength is still up to 3.98 after 15 thermal cycles. MPa significantly improves the connection performance of carbon/carbon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081608A_ABST
    Figure CN119081608A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a graphene reinforced resin-based laminated high-temperature adhesive for a carbon / carbon material, which comprises the following steps: prefabricating a gum base solution by using isopropanol and epoxy resin, adding polyethylene glycol, sodium dodecyl benzene sulfonate and ferrocene into the gum base solution according to a certain proportion to prepare adhesive cement; preparing flake graphene, and mixing the flake graphene with the adhesive cement according to a specific proportion to prepare the high-temperature adhesive. The high-temperature adhesive has the advantages that the high-temperature adhesive is high in pertinence, suitable for bonding carbon / carbon composite materials and good in interface adhesion; the bonding effect after high-temperature treatment is excellent, and the bonding strength of 3 MPa can be provided within the range of 800-1300 DEG C; the thermal cycle resistance is good, the bonding strength is increased along with the increase of the number of thermal cycles, and the strength can reach 3.98 MPa after 15 times of thermal cycles within the range of room temperature to 1300 DEG C. A large number of carbon nanotubes are generated in the graphene sheet layer on the surface of the high-temperature glue lamination layer, and the integrity retention degree of the lamination layer structure is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive material preparation, and in particular to a method for preparing a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials. Background Art

[0002] At present, the development direction of bonding technology is mainly to continuously improve and enhance the quality of bonding, reduce costs, improve production efficiency, and explore and develop aviation bonding technology suitable for new materials and new structures. In the context of the increasing demand for lightweight and environmental protection in the aviation industry, the application of bonding will become more and more common. However, carbon / carbon composite materials widely used in the aerospace field are difficult to directly prepare large components with complex structures due to the limitations of preparation and processing technology. Therefore, connecting small carbon / carbon material parts into large and complex components is a potential post-processing process, and high-temperature resistant bonding technology is particularly suitable for the connection of carbon / carbon composite materials because of its high efficiency and convenience.

[0003] As a major means of connecting and repairing carbon / carbon materials, adhesive bonding still has a series of problems such as low bonding strength, poor thermal shock resistance, and limited high-temperature use effect, which urgently needs further improvement. The bionic nacre structure (brick-mud structure) has high strength and high toughness. It has been widely used in the field of composite material preparation and has achieved good results. However, there is no precedent for applying this bionic structure to adhesive bonding. Therefore, the design of a bionic nacre structure in the adhesive bonding process is the innovation of this work. Through literature investigation, it was found that graphene has very good chemical compatibility in resin, so we proposed a new high-temperature resistant adhesive with a bionic nacre structure using polymer as "mud" and graphene as "brick". At the same time, by in-situ growing carbon nanotubes between graphene sheets, the high bonding strength at high temperature and the improvement of the joint's thermal cycling resistance can be achieved. Summary of the invention

[0004] In order to solve the above problems, the object of the present invention is to provide a method for preparing a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials.

[0005] In order to achieve the above object, the present invention provides a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials. The method comprises the following steps performed in sequence:

[0006] 1) Weigh isopropyl alcohol and epoxy resin in a mass ratio of 30:13.5-20, add them into a clean container, and stir the solution at 250-350 r / min for 20-30 minutes at room temperature to mix the solution evenly. After stirring, let it stand overnight to obtain the lower slurry, which is placed in another container as the adhesive base liquid for later use;

[0007] 2) adding polyethylene glycol, a surfactant, sodium dodecylbenzene sulfonate, and a catalyst, ferrocene, to the adhesive base liquid prepared in step (1) in a mass ratio of 1 to 2: 0.020 to 0.025: 2 to 3: 20 to 25, and sealing the container. At room temperature, mechanically stirring at 400 to 700 r / min for 10 to 12 hours until fully mixed to obtain a uniform adhesive paste;

[0008] 3) SiC is used as a carbon source and sent into a vacuum atmosphere furnace. In an ultra-low pressure environment, SiC is heated to 1200-1450°C for high temperature treatment and kept at a constant temperature for 10-20 minutes to decompose and remove the Si element, thereby preparing a graphene film. After the film is cooled to room temperature, it is taken out and ground into powder, and the obtained graphene powder is collected for later use;

[0009] 4) adding the graphene prepared in step (3) to the uniform slurry in step (2) at a solid-liquid mass ratio of 0.02 to 0.04:1, stirring again at a speed of 400 to 700 r / min for 10 to 12 hours to fully disperse the graphene in the slurry. The container needs to be sealed during the whole process, and finally the desired high-temperature adhesive is obtained.

[0010] Preferably, the isopropanol solvent in step (1) is analytically pure, with a purity higher than 99%, and is a conventional chemical that can be directly purchased; the epoxy resin is an industrial raw material, such as E51, E44, etc.

[0011] Preferably, the polyethylene glycol, sodium dodecylbenzene sulfonate and ferrocene in step (2) are all analytically pure products, and the purity needs to be higher than 99%.

[0012] Preferably, the specific stirring speed in steps (1) and (2) is determined according to the viscosity of the mixed solution. If the viscosity of the solution is high, the speed is low and the time is long; if the viscosity is low, the speed is high and the time is short.

[0013] Preferably, the SiC added in step (3) is generally single crystals such as 6H-SiC, 4H-SiC, etc. as a carbon source.

[0014] Preferably, the ultra-low pressure environment treatment method in step (3) is to first evacuate the vacuum atmosphere furnace to a pressure not higher than 3×10 -3 Pa, and then argon is introduced to a pressure not less than 0.01 MPa to protect the SiC and graphene films.

[0015] Preferably, steps (1), (2), (3) and (4) are all carried out at room temperature, and the container needs to be sealed during the entire process to prevent the slurry from volatilizing and affecting properties such as viscosity.

[0016] The present invention provides a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials having the following characteristics:

[0017] Beneficial effects:

[0018] 1. This high temperature adhesive is highly targeted and suitable for bonding carbon / carbon composite materials, and has good interface adhesion. After the high temperature adhesive is applied and dried, the adhesive layer on the surface of the sample is similar and has no major defects.

[0019] 2. This high temperature adhesive has excellent bonding effect under high temperature treatment. After curing at 250℃, the bonding strength can reach up to 10.74MPa, and it can provide 3MPa bonding strength in the range of 800~1300℃.

[0020] 3. This high temperature adhesive has good resistance to thermal cycles. In the thermal cycle from room temperature to 1300℃, its bonding strength increases with the increase in the number of thermal cycles. The strength of the high temperature resistant adhesive reaches 3.34MPa after 5 thermal cycles, 3.9MPa after 10 thermal cycles, and 3.98MPa after 15 thermal cycles.

[0021] 4. By observing the morphology of the surface of the high-temperature resistant adhesive laminate, it can be clearly seen that a large number of carbon nanotubes have grown in the graphene sheets, which has made an innovative breakthrough in further research on the in-situ growth of carbon nanotubes in graphene sheets to enhance the bonding effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a load-fracture displacement curve of the carbon / carbon material prepared in Example 1 after being treated with a graphene-reinforced resin-based laminated high-temperature adhesive at 800°C.

[0023] Figure 2 The bonding strength of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials prepared in Example 1 at different processing temperatures.

[0024] Figure 3 This is a line graph of the bonding strength of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials prepared in Example 1 after different numbers of thermal cycles in the range of room temperature to 1300°C.

[0025] Figure 4 XRD patterns of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials prepared in Example 1 after being treated at different temperatures.

[0026] Figure 5 This is an infrared spectrum of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials prepared in Example 1 after being treated at different temperatures.

[0027] Figure 6 This is the cross-sectional microscopic morphology of the adhesive layer of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials prepared in Example 1 after heat treatment at 1300°C.

[0028] Figure 7 The microscopic morphology of the surface of the laminated adhesive treated with the graphene-reinforced resin-based high-temperature adhesive for the carbon / carbon material prepared in Example 1 at 1300°C is shown in (a) low-magnification; (b) high-magnification. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] The present invention provides a technical solution: a method for preparing a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials, which specifically comprises the following steps:

[0032] 1) Weigh isopropyl alcohol and epoxy resin in a mass ratio of 30:20, add them into a clean container, and stir the solution evenly at 350r / min at room temperature for 30 minutes. After stirring, let it stand overnight to obtain the lower slurry, which is placed in another container as the adhesive base liquid for later use.

[0033] 2) Adding the bonding strengthening phase polyethylene glycol, the surfactant sodium dodecylbenzene sulfonate, and the catalyst ferrocene to the adhesive base liquid prepared in step (1) in a mass ratio of 2:0.025:2:25, and sealing the container. At room temperature, mechanical stirring is performed at 400 r / min for 12 h until it is fully mixed to obtain a uniform slurry.

[0034] 3) SiC is used as a carbon source and sent into a vacuum atmosphere furnace. In an ultra-low pressure environment, SiC is heated to 1450°C for high temperature treatment and kept at a constant temperature for 20 minutes to decompose and remove the Si element, thereby preparing a graphene film. After cooling to room temperature, the film is taken out and ground into powder, and the obtained graphene powder is collected for later use.

[0035] 4) Add 1.0 g of graphene to the uniform slurry in step (2), and stir again at a speed of 400 r / min for 12 h to fully disperse the graphene in the slurry. The container needs to be sealed during the whole process, and finally the desired high temperature resistant glue is obtained.

[0036] Example 2

[0037] 1) Weigh isopropyl alcohol and epoxy resin in a mass ratio of 30:13.5, add them into a clean container, and stir the solution at 300r / min for 20 minutes at room temperature to mix the solution evenly. After stirring, let it stand overnight to obtain the lower slurry, which is placed in another container as the adhesive base liquid for later use.

[0038] 2) Adding the bonding strengthening phase polyethylene glycol, the surfactant sodium dodecylbenzene sulfonate, and the catalyst ferrocene to the adhesive base liquid prepared in step (1) in a mass ratio of 1.5:0.020:2:20, and sealing the container. At room temperature, mechanical stirring is performed at 500 r / min for 11 hours until it is fully mixed to obtain a uniform slurry.

[0039] 3) SiC is used as a carbon source and sent into a vacuum atmosphere furnace. In an ultra-low pressure environment, SiC is heated to 1300°C for high temperature treatment and kept at a constant temperature for 10 minutes to decompose and remove the Si element, thereby preparing a graphene film. After cooling to room temperature, the film is taken out and ground into powder, and the obtained graphene powder is collected for later use.

[0040] 4) Add 0.8 g of graphene to the uniform slurry in step (2), and stir again at a speed of 500 r / min for 11 h to fully disperse the graphene in the slurry. The container needs to be sealed during the whole process, and finally the desired high temperature resistant glue is obtained.

[0041] Example 3

[0042] 1) Weigh isopropyl alcohol and epoxy resin in a mass ratio of 30:15, add them into a clean container, and stir the solution at 250r / min for 25 minutes at room temperature to mix the solution evenly. After stirring, let it stand overnight to obtain the lower slurry, which is placed in another container as the adhesive base liquid for later use.

[0043] 2) Adding the bonding strengthening phase polyethylene glycol, the surfactant sodium dodecylbenzene sulfonate, and the catalyst ferrocene to the adhesive base liquid prepared in step (1) in a mass ratio of 1.5:0.023:2.5:23, and sealing the container. At room temperature, mechanical stirring is performed at 700 r / min for 10 h until fully mixed to obtain a uniform slurry.

[0044] 3) SiC is used as a carbon source and sent into a vacuum atmosphere furnace. In an ultra-low pressure environment, SiC is heated to 1200°C for high temperature treatment and kept at a constant temperature for 15 minutes to decompose and remove the Si element, thereby preparing a graphene film. After cooling to room temperature, the film is taken out and ground into powder, and the obtained graphene powder is collected for later use.

[0045] 4) Add 0.6 g of graphene to the uniform slurry in step (2), and stir again at a speed of 700 r / min for 10 h to fully disperse the graphene in the slurry. The container needs to be sealed during the whole process, and finally the desired high temperature resistant glue is obtained.

[0046] In the preparation method of a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials provided by the present invention, flaky graphene is mainly used as "bricks" and a polymer substrate is used as "mud". A bionic pearl layer structure is applied in the adhesive layer to enhance the overall strength of the high-temperature resistant adhesive. At the same time, carbon nanotubes are grown in the graphene layer by ferrocene catalysis to achieve the connection between carbon / carbon materials. The traditional toughening method of adding a third phase not only cannot guarantee the improvement of the high-temperature adhesive effect, but greatly increases the cost. Applying low-cost in-situ growth technology to the toughening of high-temperature adhesives can not only obtain a highly uniform composite structure, but also guarantee the toughening effect with a greater probability. The addition of graphene has a good effect on improving the strength of the material. Flaky graphene is a main skeleton material for preparing a high-strength and high-toughness laminated structure, which provides a new idea for the preparation of a new type of high-temperature resistant adhesive. The high-temperature resistant adhesive was prepared using isopropyl alcohol as the solvent, sodium dodecylbenzene sulfonate as the surfactant, ferrocene as the catalyst, flaky graphene as the stacking skeleton, and epoxy resin as the bonding phase. This has made innovative breakthroughs and provided detailed data support for the further research on the application of brick-mud structure in the adhesive layer and the in-situ growth of carbon nanotubes using flaky graphene to enhance the bonding effect.

[0047] In order to verify the effect of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials provided in the above embodiment, the inventors conducted the following experiments:

[0048] 1) A carbon / carbon composite material plate (40 mm×10 mm×5 mm) that has been polished, cleaned and dried with alcohol is laid flat on a glass plate with the bonding surface facing upward.

[0049] 2) Apply the high temperature glue prepared in the above embodiment to each bonding surface of the carbon / carbon material plate, and then use an applicator to control the thickness of the glue layer before curing to 100μm. Then, the carbon / carbon material plates are bonded together with the bonding surfaces facing each other to form a bonded part, and the bonding area is controlled to be 20×10mm. Fix the bonded sample, dry it at room temperature for 12h, and then cure it at 250℃ for 1h.

[0050] 3) The cured bonded component is placed in a muffle furnace and calcined at different temperatures (800° C., 1000° C., 1300° C. and 1500° C.) for 1 hour to obtain a calcined bonded component.

[0051] 4) Room temperature shear test: The approximate shear strength of the bonded parts after being treated at different temperatures was tested using a CSS-44001 universal testing machine to evaluate the high temperature bonding effect of the high temperature adhesive prepared in Example 1 on carbon / carbon materials. Figure 1 The load-fracture displacement curve of graphene-reinforced resin-based laminated high-temperature adhesive bonded parts after treatment at 800°C is shown. Figure 2 Shown is the bond strength of the high temperature adhesive at different processing temperatures.

[0052] Depend on Figure 1 It can be seen that the load-fracture displacement curve is an upward curve as a whole, the slope of the curve is relatively high and smooth, and the shear force after fracture drops sharply, indicating that the stiffness of the adhesive layer is relatively high.

[0053] Depend on Figure 2 It can be seen that the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials has a maximum bonding strength of 10.74MPa after curing at 250°C, and can provide a bonding strength of 3MPa in the range of 800-1300°C, and has excellent bonding effect under high-temperature treatment.

[0054] 5) Thermal cycle resistance test: In addition to being able to withstand high temperatures, thermal cycle resistance is also an important indicator of high temperature adhesives. The high temperature adhesive prepared in the above embodiment was subjected to a bonding process of drying at 80°C after one coating and curing at 250°C after bonding. It was calcined at 1300°C for thermal cycle experiments. The number of thermal cycles was 5, 10, and 15 times respectively. The bonding strength of the adhesive after different thermal cycles (5, 10, and 15 times) is shown in Figure 2. Figure 3 shown.

[0055] Depend on Figure 3 It can be seen that the shear strength of the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials reaches more than 3 MPa after multiple thermal cycles, and the highest strength after 15 thermal cycles is 3.98 MPa. The shear strength slowly increases with the number of thermal cycles, proving that the high-temperature resistant adhesive prepared in the embodiment has good thermal cycle resistance.

[0056] 6) Analysis of high temperature adhesive composition: The adhesive layer treated at 800℃, 1000℃, 1300℃ and 1500℃ was ground into powder, and then the composition of the high temperature adhesive was analyzed using a D / Max 2500v / PC XRD tester. The XRD patterns of the high temperature adhesive treated at 800℃, 1000℃, 1300℃ and 1500℃ are as follows: Figure 4 shown.

[0057] Depend on Figure 4 It can be seen that after comparing with the diffraction peak standard card, it is found that the "a" diffraction peak corresponds to the laminated skeleton of the high-temperature adhesive - graphene. In addition to graphene, the appearance of the "a" peak also has the effect of cracking carbon. In addition, Figure 2A small diffraction peak "b" appears on the spectrum of the high temperature glue treated at 1500℃, and its corresponding component is SiC. This is due to the reaction between a small amount of carbon in the high temperature resistant glue and the cracked silicon.

[0058] 7) Infrared spectrum diffraction test of high temperature adhesive: The molecular structure and chemical composition of the high temperature adhesive in Example 1 were analyzed using a Nicolet TMIS10 infrared diffractometer. Figure 5 shown.

[0059] Depend on Figure 5 It can be seen that in the figure, the wavelength is 725cm -1 There is a group of absorption peaks near and around it, and it is inferred that its bonding composition is C=C, ortho-disubstituted benzene ring and CH bond; 1091cm -1 The small absorption peak near 3500-3750cm is derived from the stretching vibration of C=O bond. -1 There are absorption peaks in the region, representing NH, OH and CH bonds.

[0060] 8) Micromorphology analysis: The heat-treated bonded parts were made into SEM test specimens, and the micromorphology of the cross section of the bonded parts was observed using a Nanosem430 scanning electron microscope analyzer. Figure 6 This is the cross-sectional microscopic morphology of the adhesive layer of the high temperature resistant adhesive after heat treatment at 1300℃. Figure 7 This is the microscopic morphology of the lateral surface of the adhesive at 1300℃.

[0061] Depend on Figure 6 It can be seen that after the sample was heat treated at 1300℃, the bond between the glue layer and the carbon fiber was tight and the glue layer was dense. The graphene flakes in the glue layer also formed a stacked structure in a relatively orderly manner. Due to the influence of the observation angle and the polishing process, it is difficult to see whether carbon nanotubes exist through the microscopic morphology of the cross section.

[0062] Depend on Figure 7 It can be seen that at 1300°C, the surface of the high-temperature resistant rubber sample is relatively complete. Under high magnification, a large number of linear objects can be clearly seen, that is, catalytically generated carbon nanotubes. The number is large and the distribution is dense, indicating that 1300°C is more suitable for the growth temperature range of carbon nanotubes, which is beneficial to enhancing the strength and toughness of the material structure.

Claims

1. A method for preparing a graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials, characterized in that: The preparation method comprises the following steps performed in sequence: 1) Weigh isopropyl alcohol and epoxy resin in a mass ratio of 30:13.5-20, add them into a clean container, and stir the solution at 250-350 r / min for 20-30 minutes at room temperature to mix the solution evenly. After stirring, let it stand overnight to obtain the lower slurry, which is placed in another container as the adhesive base liquid for later use; 2) adding polyethylene glycol, a surfactant, sodium dodecylbenzene sulfonate, and a catalyst, ferrocene, to the adhesive base liquid prepared in step (1) in a mass ratio of 1 to 2: 0.020 to 0.025: 2 to 3: 20 to 25, and sealing the container. At room temperature, mechanically stirring at 400 to 700 r / min for 10 to 12 hours until fully mixed to obtain a uniform adhesive paste; 3) SiC is used as a carbon source and sent into a vacuum atmosphere furnace. In an ultra-low pressure environment, SiC is heated to 1200-1450°C for high temperature treatment and kept at a constant temperature for 10-20 minutes to decompose and remove the Si element, thereby preparing a graphene film. After the film is cooled to room temperature, it is taken out and ground into powder, and the obtained graphene powder is collected for later use; 4) adding the graphene prepared in step (3) to the uniform slurry in step (2) at a solid-liquid mass ratio of 0.02 to 0.04:1, stirring again at a speed of 400 to 700 r / min for 10 to 12 hours to fully disperse the graphene in the slurry. The container needs to be sealed during the whole process, and finally the desired high-temperature adhesive is obtained.

2. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: The isopropanol solvent in step (1) is analytically pure, with a purity higher than 99%, and is a conventional chemical that can be purchased directly; the epoxy resin is an industrial raw material, such as E51, E44, etc.

3. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: The polyethylene glycol, sodium dodecylbenzene sulfonate and ferrocene in step (2) are all analytically pure products, and the purity needs to be higher than 99%.

4. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: The specific stirring speed in steps (1) and (2) is determined by the viscosity of the mixed solution. If the solution has a high viscosity, the speed is low and the time is long; if the solution has a low viscosity, the speed is high and the time is short.

5. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: The SiC added in step (3) is generally a single crystal of 6H-SiC, 4H-SiC, etc. as a carbon source.

6. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: The method for treating the ultra-low pressure environment in step (3) is to first evacuate the vacuum atmosphere furnace to a pressure not higher than 3×10 - 3 Pa, and then argon is introduced to a pressure not less than 0.01 MPa to protect the SiC and graphene films.

7. The method for preparing the graphene-reinforced resin-based laminated high-temperature adhesive for carbon / carbon materials according to claim 1, characterized in that: Steps (1), (2), (3) and (4) are all carried out at room temperature. The container must be sealed during the entire process to prevent the slurry from volatilizing and affecting properties such as viscosity.