Epoxy repair adhesive for repairing holes in surface of carbon fiber product and preparation method of epoxy repair adhesive
By using bisphenol A and bisphenol F epoxy resins on the surface of carbon fiber products combined with isocyanate modified epoxy resins and other materials, the problem of hole damage on the surface of carbon fiber products is solved, and its weather resistance is improved. Mechanical strength extends service life and reduces the impact of friction resistance.
Patent Information
- Application Number
- CN202411334999.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-06
AI Technical Summary
Carbon fiber products are prone to surface holes and damage when used in long-term water, resulting in increased resistance and reduced performance. It is difficult for the prior art to effectively repair and improve their weather resistance and mechanical strength.
Using bisphenol A and bisphenol F type epoxy resin as the main body, isocyanate modified epoxy resin, toughener, filler and amine curing agent are added to form a five-membered heterocyclic structure and a tight network through a special preparation method to enhance the Interface bonding force and mechanical strength, and evenly disperse the material through three rollers to improve adhesion and smooth and bright surface.
Effectively improve the weather resistance, impact toughness and mechanical strength of carbon fiber products surface repair glue, extend service life, reduce the influence of friction resistance, and improve overall performance.
Smart Images

Figure BDA0005058020620000021 
Figure BDA0005058020620000061 
Figure BDA0005058020620000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin adhesives, and in particular to an epoxy repair adhesive for repairing holes on the surface of a carbon fiber product and a preparation method thereof. Background Art
[0002] Carbon fiber products refer to products made of carbon fiber prepreg cloth as raw materials, which are processed into materials that meet the requirements of use through different processing methods. Processing methods of carbon fiber products: winding, rolling, molding, vacuum forming, inflation molding, etc. Civilian carbon fiber products are mostly made by rolling, molding, vacuum forming, and inflation molding. Carbon fiber is light in weight and carbon fiber products have high strength, far exceeding metal materials of the same volume and weight. Due to the high strength characteristics of carbon fiber, carbon fiber products have extremely high hardness. Carbon fiber products are widely used in many fields due to their excellent performance.
[0003] Carbon fiber products, such as carbon fiber hydrofoils, are underwater wing-shaped structures made of carbon fiber composite materials and are widely used in water sports equipment, ships and other water vehicles. Since carbon fiber hydrofoils are subject to water erosion when used in water for a long time, they are prone to surface holes and damage, which can easily lead to increased resistance and overall performance degradation or damage of carbon fiber hydrofoils during use. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, one of the purposes of the present invention is to provide an epoxy repair adhesive for repairing holes on the surface of carbon fiber products.
[0005] The second object of the present invention is to provide a method for preparing an epoxy repair adhesive for repairing holes on the surface of a carbon fiber product. The preparation method is simple to operate, convenient to control, high in production efficiency, low in production cost, and can be used for large-scale production.
[0006] One of the purposes of the present invention is achieved through the following technical solution: An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product comprises the following raw materials in parts by weight:
[0007] 30-50 parts of bisphenol A epoxy resin
[0008] Bisphenol F epoxy resin 20-40 parts
[0009]
[0010] The epoxy repair glue for repairing holes on the surface of carbon fiber products uses bisphenol A epoxy resin and bisphenol F epoxy resin as the main resins, maintains basic bonding strength, adds isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent, and after curing, has good adhesion effect, and can effectively improve its weather resistance, impact toughness and mechanical strength, and has a better surface smoothness and brightness. Among them, the isocyanate modified epoxy resin prepared by a special method not only gives the epoxy resin significantly enhanced thermal stability, and its heat resistance is more excellent, but also enhances the interfacial bonding force of the epoxy repair glue, has a more optimized network structure, enhances the rigidity of the epoxy resin molecular chain, can better resist the action of external forces, thereby improving the mechanical strength of the epoxy resin, and at the same time, under the action of the toughening agent, it can achieve the toughening effect and improve the mechanical strength of the epoxy repair glue, and avoid the cured epoxy repair glue from being easily separated or damaged from the carbon fiber product by water erosion. In addition, the added filler and coupling agent work together to help the filler to be evenly dispersed and combined in the epoxy repair adhesive, improve the smooth and bright surface effect of the epoxy repair adhesive after curing, effectively reduce the friction resistance during use, and help extend the service life of the epoxy repair adhesive after curing, and effectively reduce the adverse effects of friction resistance on the overall performance.
[0011] Preferably, the bisphenol A epoxy resin is E44; the bisphenol F epoxy resin is NPEF-170 or BFE-170.
[0012] Preferably, the preparation method of each portion of the isocyanate-modified epoxy resin comprises the following steps:
[0013] (R1), take 100 parts of epoxy resin E44, 20-30 parts of isocyanate monomer, 0.5 parts of chain extender, 1-2 parts of plasticizer, 0.05-0.1 parts of 2-ethyl-4-methylimidazole, 1-2 parts of antioxidant and 10-15 parts of cyclohexanone by weight, and set aside;
[0014] (R2), after mixing the isocyanate monomer and the chain extender, heating to 50-60° C., stirring for 1-2 hours, to obtain an isocyanate prepolymer;
[0015] (R3), after mixing epoxy resin E44 and plasticizer and heating to 80-100° C., add isocyanate prepolymer and stir evenly to obtain a mixed solution;
[0016] (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 180-195° C. for 10-12 hours, and cooling to room temperature to obtain a reaction product;
[0017] (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
[0018] By adopting the above technical scheme, the isocyanate-modified epoxy resin is extended with isocyanate monomer and then reacted with epoxy resin E44 under the action of 2-ethyl-4-methylimidazole to generate an oxazolidinone-type five-membered heterocyclic structure, which is more stable and more conducive to improving the weather resistance of epoxy resin. The isocyanate monomer chain extension promotes the cross-linking reaction of the epoxy resin, increases the cross-linking density, helps to form a more compact and stable network structure, further improves the weather resistance of the epoxy resin, and can better disperse and withstand external forces, reduce the occurrence of stress concentration, and improve the overall mechanical strength of the material; and the formation of the five-membered heterocyclic structure enhances the rigidity of the epoxy resin molecular chain, which can better resist the action of external forces, is not easy to deform and damage, thereby improving the mechanical strength of the epoxy resin, and also enhances the interface bonding force together with the filler, so that the epoxy repair glue can work better together when subjected to external forces and resist damage together. The added plasticizer effectively improves the flexibility of the isocyanate-modified epoxy resin during the preparation process, reduces its stress during long-term exposure to the environment, and thus works together with the antioxidant and isocyanate to further improve its weather resistance.
[0019] Preferably, the isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 5-8:1.
[0020] By adopting the above technical solution, diphenylmethane-4,4'-diisocyanate and toluene diisocyanate are jointly modified, which is more conducive to optimizing the cross-linking structure, further improving the heat resistance of the material, and also making the epoxy repair adhesive more stable when bearing loads.
[0021] Preferably, the plasticizer is tricresyl phosphate or epoxy soybean oil; the chain extender is 1,4-butanediol or ethylenediamine; the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:1. The above plasticizer is used to effectively improve the flexibility of the isocyanate-modified epoxy resin during the preparation process, reduce its stress during long-term exposure to the environment, and thus work together with the above antioxidant and the isocyanate after chain extension to further improve its weather resistance.
[0022] Preferably, the toughening agent is a mixture of phthalazine copoly(arylethersulfone) powder and sulfonated lignin powder in a weight ratio of 3-5:2.
[0023] By adopting the above technical scheme, the synergistic effect of poly(phenylene ether sulfone) powder (PPBES) and sulfonated lignin is more conducive to improving the overall toughening effect. Among them, poly(phenylene ether sulfone) powder has good compatibility in epoxy repair glue and forms a strong interface bond, which is more capable of preventing cracks from spreading further and more effectively improving the impact strength of the cured product; sulfonated lignin powder can form an effective interaction with epoxy resin in epoxy repair glue through its unique molecular structure and chemical properties, thereby improving the toughness of the material. The epoxy repair glue is filled in the cracks or defects on the surface of the product, and the sulfonated lignin powder plays a bridging and reinforcing role, preventing the expansion of cracks and the destruction of materials, and improving the overall toughness. In addition, the sulfonated lignin powder and the coupling agent can jointly reduce the surface tension between the filler particles, reduce the agglomeration phenomenon between the filler particles, and make the filler more evenly distributed in the matrix. Due to the polarity of lignin, the sulfonated lignin enhances the interfacial bonding between the filler and the epoxy resin, further improving the overall performance of the epoxy repair glue.
[0024] Preferably, the filler is at least one of talcum powder, fumed silica, nano silicon carbide and diatomaceous earth; and the coupling agent is KH-560 or KH-570.
[0025] Using the above technical solution, more preferably, the filler is a mixture of talcum powder, fumed silica and nano-silicon carbide in a weight ratio of 1:3-5:1. Under the joint action of sulfonated lignin powder and coupling agent, the above filler compound is applied to the epoxy repair glue, which has a strong reinforcing effect and can significantly improve the rheological properties of the repair glue, making the structure of the material denser, reducing pores and defects, making it more stable during the construction process and not easy to sag, while improving the uniformity, glossiness and smoothness of the repair glue layer.
[0026] Preferably, the amine curing agent is at least one of isophorone diamine, polyetheramine D-230, polyamide 125 and polyamide 650.
[0027] The second object of the present invention is achieved by the following technical solution: The preparation method of the above-mentioned epoxy repair adhesive for repairing holes on the surface of carbon fiber products comprises the following steps:
[0028] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside;
[0029] (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
[0030] Among them, in step (S2), grinding with a three-roll mill is more conducive to grinding and uniformly dispersing system materials, improving the processing performance of materials, and enhancing the physical properties of products.
[0031] Preferably, when the epoxy repair adhesive for repairing holes on the surface of the carbon fiber product is used, the epoxy repair adhesive is applied to the surface of the carbon fiber product and then cured at room temperature for 20-30 hours, or heated to 50-60° C. and cured for 30-60 minutes.
[0032] The beneficial effects of the present invention are as follows: the epoxy repair adhesive for repairing holes on the surface of carbon fiber products of the present invention uses bisphenol A epoxy resin and bisphenol F epoxy resin as main resins, maintains basic bonding strength, and isocyanate-modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent are added. After curing, the adhesion effect is good, and the weather resistance, impact toughness and mechanical strength can be effectively improved, and the surface smoothness and brightness effect are better.
[0033] The preparation method of the invention has the advantages of simple operation, convenient control, high production efficiency and low production cost, and can be used for large-scale production. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0035] Example 1
[0036] An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product comprises the following raw materials in parts by weight:
[0037]
[0038] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is NPEF-170.
[0039] The preparation method of each isocyanate-modified epoxy resin comprises the following steps:
[0040] (R1), take 100 parts of epoxy resin E44, 25 parts of isocyanate monomer, 0.5 parts of chain extender, 1.5 parts of plasticizer, 0.08 parts of 2-ethyl-4-methylimidazole, 1.5 parts of antioxidant and 12 parts of cyclohexanone by weight, and set aside;
[0041] (R2), after mixing the isocyanate monomer and the chain extender, heating to 55° C. and stirring for 1.5 h to obtain an isocyanate prepolymer;
[0042] (R3), after mixing epoxy resin E44 and plasticizer and heating to 90° C., add isocyanate prepolymer and stir evenly to obtain a mixed solution;
[0043] (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 190° C. for 11 h, then cooling to room temperature to obtain a reaction product;
[0044] (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
[0045] The isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 6:1.
[0046] The plasticizer is epoxidized soybean oil; the chain extender is 1,4-butanediol; and the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:1.
[0047] The toughening agent is prepared by mixing phthalazine copoly(arylethersulfone) powder and sulfonated lignin powder in a weight ratio of 4:2.
[0048] The filler is a mixture of talcum powder, fumed silica and nano silicon carbide in a weight ratio of 1:4:1; and the coupling agent is KH-560.
[0049] The amine curing agent is prepared by mixing isophorone diamine, polyetheramine D-230 and polyamide 650 in a weight ratio of 2.5:1:1.
[0050] The preparation method of the epoxy repair adhesive for repairing holes on the surface of carbon fiber products comprises the following steps:
[0051] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside;
[0052] (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
[0053] Example 2
[0054] An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product comprises the following raw materials in parts by weight:
[0055]
[0056] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is NPEF-170.
[0057] The preparation method of each isocyanate-modified epoxy resin comprises the following steps:
[0058] (R1), take 100 parts of epoxy resin E44, 20 parts of isocyanate monomer, 0.5 parts of chain extender, 1 part of plasticizer, 0.05 parts of 2-ethyl-4-methylimidazole, 1 part of antioxidant and 10 parts of cyclohexanone by weight, and set aside;
[0059] (R2), after mixing the isocyanate monomer and the chain extender, heating to 50° C. and stirring for 1 hour to obtain an isocyanate prepolymer;
[0060] (R3), after mixing epoxy resin E44 and plasticizer and heating to 80° C., adding isocyanate prepolymer and stirring evenly to obtain a mixed solution;
[0061] (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 195° C. for 10 h, then cooling to room temperature to obtain a reaction product;
[0062] (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
[0063] The isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 5:1.
[0064] The plasticizer is epoxidized soybean oil; the chain extender is 1,4-butanediol; and the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:1.
[0065] The toughening agent is prepared by mixing phthalazinone copolyarylethersulfone powder and sulfonated lignin powder in a weight ratio of 3:2.
[0066] The filler is a mixture of talcum powder, fumed silica and nano silicon carbide in a weight ratio of 1:3:1; and the coupling agent is KH-560.
[0067] The amine curing agent is prepared by mixing isophorone diamine, polyetheramine D-230 and polyamide 650 in a weight ratio of 2:1:1.
[0068] The preparation method of the epoxy repair adhesive for repairing holes on the surface of carbon fiber products comprises the following steps:
[0069] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside;
[0070] (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
[0071] Example 3
[0072] An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product comprises the following raw materials in parts by weight:
[0073]
[0074] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is NPEF-170.
[0075] The preparation method of each isocyanate-modified epoxy resin comprises the following steps:
[0076] (R1), take 100 parts of epoxy resin E44, 30 parts of isocyanate monomer, 0.5 parts of chain extender, 2 parts of plasticizer, 0.1 parts of 2-ethyl-4-methylimidazole, 2 parts of antioxidant and 15 parts of cyclohexanone by weight, and set aside;
[0077] (R2), after mixing the isocyanate monomer and the chain extender, heating to 60° C. and stirring for 2 h to obtain an isocyanate prepolymer;
[0078] (R3), after mixing epoxy resin E44 and plasticizer and heating to 100° C., adding isocyanate prepolymer and stirring evenly to obtain a mixed solution;
[0079] (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 180° C. for 12 h, then cooling to room temperature to obtain a reaction product;
[0080] (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
[0081] The isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 8:1.
[0082] The plasticizer is epoxidized soybean oil; the chain extender is 1,4-butanediol; and the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:1.
[0083] The toughening agent is prepared by mixing phthalazine copoly(arylethersulfone) powder and sulfonated lignin powder in a weight ratio of 5:2.
[0084] The filler is a mixture of talcum powder, fumed silica and nano silicon carbide in a weight ratio of 1:5:1; and the coupling agent is KH-560.
[0085] The amine curing agent is prepared by mixing isophorone diamine, polyetheramine D-230 and polyamide 650 in a weight ratio of 3:1:1.
[0086] The preparation method of the epoxy repair adhesive for repairing holes on the surface of carbon fiber products comprises the following steps:
[0087] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside;
[0088] (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
[0089] Example 4
[0090] An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product comprises the following raw materials in parts by weight:
[0091]
[0092]
[0093] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is NPEF-170.
[0094] The preparation method of each isocyanate-modified epoxy resin comprises the following steps:
[0095] (R1), take 100 parts of epoxy resin E44, 27 parts of isocyanate monomer, 0.5 parts of chain extender, 1.8 parts of plasticizer, 0.06 parts of 2-ethyl-4-methylimidazole, 1.2 parts of antioxidant and 14 parts of cyclohexanone by weight, and set aside;
[0096] (R2), after mixing the isocyanate monomer and the chain extender, heating to 58° C. and stirring for 1.2 h to obtain an isocyanate prepolymer;
[0097] (R3), after mixing epoxy resin E44 and plasticizer and heating to 95° C., adding isocyanate prepolymer and stirring evenly to obtain a mixed solution;
[0098] (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 190° C. for 11 h, and cooling to room temperature to obtain a reaction product;
[0099] (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
[0100] The isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 7:1.
[0101] The plasticizer is epoxidized soybean oil; the chain extender is 1,4-butanediol; and the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:1.
[0102] The toughening agent is prepared by mixing phthalazine copoly(arylethersulfone) powder and sulfonated lignin powder in a weight ratio of 4:2.
[0103] The filler is a mixture of talcum powder, fumed silica and nano silicon carbide in a weight ratio of 1:5:1; and the coupling agent is KH-560.
[0104] The amine curing agent is prepared by mixing isophorone diamine, polyetheramine D-230 and polyamide 650 in a weight ratio of 2.8:1:1.
[0105] The preparation method of the epoxy repair adhesive for repairing holes on the surface of carbon fiber products comprises the following steps:
[0106] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside;
[0107] (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
[0108] Comparative Example 1
[0109] The difference between this comparative example and Example 1 is:
[0110] The isocyanate-modified epoxy resin is replaced by polyurethane-modified epoxy resin EPU-300A.
[0111] Comparative Example 2
[0112] The difference between this comparative example and Example 1 is:
[0113] In the preparation method of each part of the isocyanate-modified epoxy resin, the weight parts of the raw materials are 100 parts of epoxy resin E44, 25 parts of isocyanate monomer, 0.5 parts of chain extender, 0 parts of plasticizer, 0.08 parts of 2-ethyl-4-methylimidazole, 3 parts of antioxidant and 12 parts of cyclohexanone. That is, the content of plasticizer in the isocyanate-modified epoxy resin is 0.
[0114] Comparative Example 3
[0115] The difference between this comparative example and Example 1 is:
[0116] The toughening agent is a mixture of styrene-butadiene rubber powder and TPU toughening agent in a weight ratio of 4:2.
[0117] Comparative Example 4
[0118] The difference between this comparative example and Example 1 is:
[0119] The filler is a mixture of calcium carbonate and silicon dioxide in a weight ratio of 1:4.
[0120] Performance Testing
[0121] Take the epoxy repair adhesive of Example 1-4 and Comparative Example 1-4, the curing condition of the epoxy repair adhesive is curing at room temperature for 24 hours, and perform tensile strength, impact resistance, weather resistance, adhesion and surface roughness tests. The test method is as follows:
[0122] Tensile strength: Tested in accordance with the provisions of GB / T2567-2008, the tensile strength is measured in MPa;
[0123] Impact resistance: According to the provisions of GB / T2567-2008 simply supported beam impact toughness test, the impact strength is measured in kJ / m 2 ;
[0124] Weather resistance: According to the provisions of the simply supported beam impact toughness test of GB / T2567-2008, a type I specimen is used and placed in a constant temperature and humidity test chamber at a temperature of 85 degrees Celsius and a humidity of 85% for 168 hours. The specimen is taken out for testing and its impact strength is tested in kJ / m 2
[0125] Adhesion: Adhesion test is carried out and its grade is assessed according to GB / T9286-1998. The base material of the sample is the cured carbon fiber prepreg.
[0126] Surface roughness Ra: Surface roughness Ra is tested according to GB1031-2009 standard, in μm;
[0127] The test results are shown in Table 1 below:
[0128]
[0129] As can be seen from Table 1 above, the epoxy repair glue for repairing holes on the surface of carbon fiber products of the present invention uses bisphenol A epoxy resin and bisphenol F epoxy resin as the main resins, maintains basic bonding strength, adds isocyanate-modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent, and after curing, has good adhesion effect, and can effectively improve its weather resistance, impact toughness and mechanical strength, and the surface is smooth and bright. The effect is better. Among them, the isocyanate-modified epoxy resin prepared by a special method not only gives the epoxy resin significantly enhanced thermal stability, its heat resistance is more excellent, but also enhances the interfacial bonding force of the epoxy repair glue, has a more optimized network structure, enhances the rigidity of the epoxy resin molecular chain, can better resist the effect of external forces, thereby improving the mechanical strength of the epoxy resin, and under the action of the toughening agent, the toughening effect is achieved and the mechanical strength of the epoxy repair glue is improved, so as to avoid the cured epoxy repair glue being easily separated or damaged from the carbon fiber product by water scouring. In addition, the added filler and coupling agent work together to help the filler to be evenly dispersed and combined in the epoxy repair adhesive, improve the smooth and bright surface effect of the epoxy repair adhesive after curing, effectively reduce the friction resistance during use, and help extend the service life of the epoxy repair adhesive after curing, and effectively reduce the adverse effects of friction resistance on the overall performance.
[0130] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. An epoxy repair adhesive for repairing holes on the surface of a carbon fiber product, characterized in that: The invention comprises the following raw materials in parts by weight:
2. The epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 1, characterized in that: The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is NPEF-170 or BFE-170.
3. The epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 1, characterized in that: The preparation method of each isocyanate-modified epoxy resin comprises the following steps: (R1), take 100 parts of epoxy resin E44, 20-30 parts of isocyanate monomer, 0.5 parts of chain extender, 1-2 parts of plasticizer, 0.05-0.1 parts of 2-ethyl-4-methylimidazole, 1-2 parts of antioxidant and 10-15 parts of cyclohexanone by weight, and set aside; (R2), after mixing the isocyanate monomer and the chain extender, heating to 50-60° C., stirring for 1-2 hours, to obtain an isocyanate prepolymer; (R3), after mixing epoxy resin E44 and plasticizer and heating to 80-100° C., add isocyanate prepolymer and stir evenly to obtain a mixed solution; (R4), adding 2-ethyl-4-methylimidazole to the mixed solution, continuing stirring and reacting at 180-195° C. for 10-12 hours, and cooling to room temperature to obtain a reaction product; (R5) adding cyclohexanone and an antioxidant to the reaction product and mixing them evenly to obtain an isocyanate-modified epoxy resin.
4. The epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 3, characterized in that: The isocyanate monomer is a mixture of diphenylmethane-4,4'-diisocyanate and toluene diisocyanate in a weight ratio of 5-8:
1.
5. The epoxy repair adhesive for repairing holes on the surface of carbon fiber products according to claim 3, characterized in that: The plasticizer is tricresyl phosphate or epoxidized soybean oil; the chain extender is 1,4-butanediol or ethylenediamine; and the antioxidant is a mixture of V85-P and V78-P in a weight ratio of 1:
1.
6. The epoxy repair adhesive for repairing holes on the surface of carbon fiber products according to claim 1, characterized in that: The toughening agent is prepared by mixing phthalazinone copolyarylethersulfone powder and sulfonated lignin powder in a weight ratio of 3-5:
2.
7. The epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 1, characterized in that: The filler is at least one of talcum powder, fumed silica, nano silicon carbide and diatomaceous earth; and the coupling agent is KH-560 or KH-570.
8. The epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 1, characterized in that: The amine curing agent is at least one of isophorone diamine, polyetheramine D-230, polyamide 125 and polyamide 650.
9. A method for preparing the epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to any one of claims 1 to 8, characterized in that: The steps include: (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler, coupling agent and amine curing agent according to weight parts, and set aside; (S2) Mix bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanate modified epoxy resin, toughening agent, filler and coupling agent evenly, grind with a three-roll grinder, add amine curing agent and stir evenly to obtain epoxy repair glue for repairing holes on the surface of carbon fiber products.
10. The method for preparing an epoxy repair adhesive for repairing holes on the surface of a carbon fiber product according to claim 9, characterized in that: When the epoxy repair adhesive for repairing holes on the surface of the carbon fiber product is used, the epoxy repair adhesive is applied to the surface of the carbon fiber product and then cured at room temperature for 20-30 hours, or heated to 50-60° C. and cured for 30-60 minutes.
Citation Information
Patent Citations
Toughening epoxy resin composition and application thereof
CN102838843A
Epoxy resin adhesive for repairing building cracks and preparation method of epoxy resin adhesive
CN115340838A
Permeation type adhesive and method for repairing steel structure
JP2004263048A