Phase change composite material and preparation method thereof
By preparing solid interface solubilizers in modified solvents and compounding them in carbon-based porous materials, the problems of difficult and low efficiency of water-soluble phase change materials are solved, and phase change composites with high thermal conductivity and high enthalpy retention rate are achieved Material, suitable for thermal management of high-power electronic components.
Patent Information
- Application Number
- CN202411202685.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The complexing of water-soluble phase change materials in carbon-based porous materials is difficult and the composite efficiency is low, resulting in poor thermal reinforcement effect. The use of surfactants in existing methods will affect the performance of phase change materials.
By modifying the inorganic reaction precursor and nanoparticles in the modified solvent, a solid interface solubilizer is prepared and dispersed in a molten water-soluble phase change material, and water solubility is achieved using vacuum impregnation or pressure infusion technology. Large proportion of phase change materials in carbon-based porous materials.
A large proportion of water-soluble phase change materials in carbon-based materials with micron or submicron pore sizes has been realized, and the thermal conductivity is improved, with thermal conductivity above 20W/(m·K), and the enthalpy retention rate is as high as more than 70%. And the stability and properties of phase change materials were not affected.
Smart Images

Figure CN119081659A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of phase change energy storage materials, and specifically relates to a method for preparing a phase change composite material by compounding a water-soluble phase change material in a carbon-based porous material, and the phase change composite material prepared thereby. Background Art
[0002] In recent years, with the vigorous development of the electronics industry, high-power electronic components have been widely used in various types of electronic equipment. Due to the severe limitation of the internal space of electronic equipment, how to achieve rapid cooling of high-power electronic devices has become a key issue for scientific researchers.
[0003] Phase change material is a type of material that can responsively absorb or release energy from the outside world in the form of latent heat through phase change. It has good energy storage (including cold storage and heat storage) performance and has been widely used in new energy, building energy conservation, industrial waste heat recovery and other fields in recent years.
[0004] Although phase change materials have good temperature control performance, their thermal conductivity is low, usually 0.2 to 0.4 W / (m·K), which is difficult to meet the needs of rapid cooling of high-power electronic components. Therefore, they need to be subjected to thermal conductivity enhancement treatment.
[0005] The traditional method of heat conductivity enhancement is to disperse metal particles with high thermal conductivity in the molten phase change material. However, the problem with this traditional treatment method is that it is difficult for metal particles to maintain stable dispersion in the phase change material. With the recycling of the phase change material, sedimentation will occur. At the same time, it is difficult for metal particles to form a three-dimensional network structure in the phase change material, and the heat conductivity enhancement effect is poor.
[0006] Another way to enhance the thermal conductivity of phase change materials is to use a thermally conductive skeleton with a porous structure. This thermally conductive skeleton has a stable structure, and its network structure can significantly improve the thermal conductivity of phase change materials, so it has become a popular material for enhancing the thermal conductivity of phase change materials in recent years.
[0007] In recent years, patents have been published on the technology of enhancing the thermal conductivity of phase change materials by using a thermally conductive skeleton with a porous structure. According to the composition classification, it can be generally divided into a metal porous skeleton and a carbon-based porous skeleton.
[0008] Metal porous skeleton materials are represented by copper foam, which have large pore sizes, mostly in the millimeter level, and can realize large-scale compounding of most phase change materials. However, the large pore size of metal porous skeleton materials also leads to a small thermal conductivity skeleton density and a weak thermal conductivity enhancement effect.
[0009] The pore size of porous carbon-based materials is at the nanometer or micrometer level, and has an excellent thermal conductivity enhancement effect. However, because the base pore size of porous carbon-based materials is too small, when the surface properties of phase change materials (such as water-soluble phase change materials) are greatly different from those of porous carbon-based materials, it is difficult for phase change materials to infiltrate the surface of porous carbon-based materials, which will directly affect the composite efficiency and greatly reduce the thermal conductivity enhancement effect.
[0010] Some people have proposed using surfactants to solve the problem of difficult wetting of phase change materials and porous carbon-based materials, which affects the composite efficiency. However, the surfactants used in this method are easily mixed into the phase change material, thus affecting the performance of the phase change composite material, especially the phase change temperature and heat absorption performance. Summary of the invention
[0011] In order to solve the problem that the water-soluble phase change material is difficult to composite and has low composite efficiency in a carbon-based porous skeleton, the present invention provides a method for preparing a phase change composite material in a first aspect, characterized in that the method comprises the following steps:
[0012] 1) in a modification solvent, allowing an inorganic reaction precursor and nanoparticles to undergo a modification reaction to achieve surface modification of the nanoparticles, and then separating and drying to obtain a solid interface solubilizer;
[0013] 2) dispersing the solid interface solubilizing agent in a molten water-soluble phase change material to obtain a phase change material blending system;
[0014] 3) immersing the carbon-based porous material in the phase change material blending system to obtain a composite impregnation material;
[0015] 4) Under the condition of vacuum impregnation or pressure infusion, the composite impregnated material is used to realize the compounding of the water-soluble phase change material in the carbon-based porous material to obtain a phase change composite material.
[0016] In a second aspect, the present invention provides a phase change composite material prepared by the method described in the first aspect of the present invention.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] (1) It is possible to realize large-scale compounding of water-soluble phase change materials in carbon-based materials with micron or submicron pore sizes.
[0019] (2) The surface modification of inorganic nanoparticles has a simple process, low cost and is easy to realize industrial production.
[0020] (3) The prepared phase change composite material has high thermal conductivity, and the thermal conductivity can reach above 20W / (m·K).
[0021] (4) The enthalpy retention rate of the prepared phase change composite material is high, which can reach more than 70%.
[0022] (5) Due to the stabilizing effect of the solid interface compatibilizer on the phase change material, the leakage rate of the phase change material in the porous material is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the carbon foam phase change composite material prepared in Example 1 of the present invention.
[0024] Figure 2 This is the DSC graph of the carbon foam phase change composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] As described above, the present invention provides a method for preparing a phase change composite material in a first aspect, characterized in that the method comprises the following steps:
[0027] 1) in a modification solvent, allowing an inorganic reaction precursor and nanoparticles to undergo a modification reaction to achieve surface modification of the nanoparticles, and then separating and drying to obtain a solid interface solubilizer;
[0028] 2) dispersing the solid interface solubilizing agent in a molten water-soluble phase change material to obtain a phase change material blending system;
[0029] 3) immersing the carbon-based porous material in the phase change material blending system to obtain a composite impregnation material;
[0030] 4) Under the condition of vacuum impregnation or pressure infusion, the composite impregnated material is used to realize the compounding of the water-soluble phase change material in the carbon-based porous material to obtain a phase change composite material.
[0031] The present invention uses an inorganic reaction precursor to modify the surface of nanoparticles so that their surfaces are modified by functional groups. The modified nanoparticles are further used as solid interface solubilizers and dispersed in molten water-soluble phase change materials. The modified nanoparticles have amphiphilicity and can optimize the wettability of the water-soluble phase change material on the surface of the carbon-based porous material, thereby improving the composite effect of the water-soluble phase change material in the micron pores of the carbon-based porous material.
[0032] In some embodiments, the inorganic reaction precursor is selected from at least one of tetra-n-butyl titanate, tetraisopropyl titanate, ethyl orthosilicate, epoxypropyl trimethoxysilane, phenyl triethoxysilane, methacryloxypropyl trimethoxysilane, methacryloxypropyl triethoxysilane, aminopropyl trimethoxysilane, aminopropyl triethoxysilane, phenyl trimethoxysilane, n-octyl triethoxysilane, tetrabutyl stannate, tetrabutyl zirconate, triisopropyl aluminate and benzyl aluminate.
[0033] In other embodiments, the nanoparticles are selected from at least one of aluminum oxide, zirconium oxide, zirconium oxide, and titanium oxide.
[0034] Preferably, the size of the nanoparticles is 1 to 100 nm (eg, 1, 5, 10, 20, 50, 100 nm), preferably 10 to 50 nm.
[0035] In other embodiments, the mass ratio of the inorganic reaction precursor to the nanoparticles is 1:0.1-100 (for example, 1:0.1, 1, 5, 10, 50 or 100), preferably 1:1-50.
[0036] In some preferred embodiments, the modified solvent is selected from at least one of water, methanol, ethanol, tetrahydrofuran and N,N-dimethylformamide.
[0037] In some preferred embodiments, the mass ratio of the modified solvent to the nanoparticles is 1:100 to 1:1000, for example, 1:100, 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900 or 1:1000.
[0038] In some preferred embodiments, the reaction temperature of the modification reaction is 10°C to 70°C (e.g., 50°C), and the reaction time is 0.5 hour to 72 hours (e.g., 0.5, 1, 3, 6, 9, 12, 24, 36, 48, 60 or 72 hours).
[0039] In some preferred embodiments, the modified nanoparticles (i.e., solid interface solubilizer particles) are separated by centrifugation, and the centrifugal speed is 3000-15000 rpm (e.g., 5000 or 10000 rpm), and the centrifugal time is 2-30 minutes (e.g., 5, 10, 15, 20, 25 or 30 minutes).
[0040] The present invention has no particular restrictions on the drying method of the nanoparticles obtained after centrifugation. For example, the nanoparticles can be dried under vacuum conditions, and the drying temperature can be above room temperature (25° C.), for example, 25° C. to 100° C. (such as 30, 40, 50, 60, 70, 80, 90 or 100° C.). The vacuum degree of vacuum drying can be -0.080 to 0.090 MPa.
[0041] In other embodiments, the water-soluble phase change material is selected from at least one of alcohol compounds and organic acid compounds.
[0042] Preferably, the alcohol compound is selected from at least one of glycerol, tetratetrol, dodecanol, tetradecanol, hexadecanol and erythritol.
[0043] It is also preferred that the organic acid compound is at least one selected from the group consisting of caprylic acid, capric acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, lauric acid, myristic acid, palmitic acid and stearic acid.
[0044] In some preferred embodiments, the dispersion is achieved by high-speed shearing. Preferably, the shear speed of the dispersion is 1000 to 25000 rpm (for example, 1000, 5000, 10000, 15000, 20000 or 25000 rpm), and the shear time is 0.5 to 30 minutes (for example, 0.5, 1, 5, 10, 15, 20 or 30 minutes).
[0045] In some preferred embodiments, the dispersion is achieved by ultrasound. Preferably, the ultrasonic frequency of the ultrasonic dispersion is 1000 Hz to 40,000 Hz (e.g., 1000, 5000, 10,000, 20,000, 30,000 or 40,000 Hz), and the ultrasonic treatment time is 10 minutes to 60 minutes (e.g., 15, 20, 25, 30, 35, 40, 45, 50, 55 or 60 minutes).
[0046] In some preferred embodiments, the dispersing may be performed at a temperature 10-40° C. higher than the melting point of the water-soluble phase change material (eg, 10, 20, 30, or 40° C. higher than the melting point of the water-soluble phase change material).
[0047] In some preferred embodiments, the mass ratio of the solid interface solubilizer to the water-soluble phase change material may be 1:100 to 1:1000, for example, 1:100, 1:200, 1:300, 1:400, 1:500, 1:600, 1:700, 1:800, 1:900 or 1:1000.
[0048] In some preferred embodiments, the carbon-based porous material is selected from at least one of carbon foam, graphene foam, expanded graphite and carbon nanotubes.
[0049] In some preferred embodiments, the compounding may be performed at a temperature 10-40° C. higher than the melting point of the water-soluble phase change material (eg, 10, 20, 30 or 40° C. higher than the melting point of the water-soluble phase change material).
[0050] In some preferred embodiments, the composite process of the phase change material and the carbon-based porous material is achieved by at least one of vacuum impregnation and pressure infusion.
[0051] In the case of a composite process using vacuum impregnation, preferably, the vacuum degree of the vacuum impregnation is -0.07 MPa to -0.095 MPa, more preferably -0.085 MPa to -0.090 MPa. The treatment time is 1 to 36 hours (e.g., 5, 10, 15, 20, 30, 36 hours).
[0052] In the case of a composite process using pressure perfusion, preferably, the pressure of the pressure perfusion is 0.10 MPa to -0.30 MPa, more preferably 0.15 MPa to 0.20 MPa. The treatment time is 1 to 36 hours (e.g., 5, 10, 15, 20, 30, 36 hours).
[0053] The present invention has no particular limitation on the amount of the carbon-based porous material and the phase change material blending system used in the composite process. Generally, the phase change material blending system can immerse the carbon-based porous material to fully impregnate it.
[0054] In the present invention, the enthalpy retention rate of the phase change composite material obtained after the thermal conductivity enhancement is consistent with the mass proportion of the water-soluble phase change material, and can be calculated by melting enthalpy or crystallization enthalpy, and the calculation method is as follows:
[0055] Enthalpy retention rate = phase change material content = ΔH m / ΔH m0 ×100%;
[0056] Where ΔH m0 is the phase change enthalpy of the water-soluble phase change material, ΔH m is the phase change point enthalpy of the phase change composite material.
[0057] In addition, the phase change temperature of the phase change composite material prepared by the method of the present invention can be 10 to 130° C. (e.g., 10, 12, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, 80, 90, 100, 110, 120 or 130° C.); preferably 20 to 125° C. The thermal conductivity of the phase change composite material can be 5 W ( / m·K) to 60 W / (m·K), preferably 20 W / (m·K) to 40 W / (m·K).
[0058] The method of the present invention utilizes modified nanoparticles as amphiphilic solid interface solubilizers to improve the wettability of the phase change material and the surface of the carbon-based porous material, thereby achieving a large-scale direct composite of the water-soluble phase change material and the carbon-based porous material. The thermal conductivity of the phase change composite material prepared by the present invention is significantly improved, and can be widely used in the field of thermal management of high-power electronic components.
[0059] Example
[0060] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content recorded in the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the present invention equally.
[0061] Example 1
[0062] Weigh 50g of SiO2 nanoparticles with a size of 50nm and add them to 500ml of methanol. Add 10g of aminopropyltriethoxysilane and 10g of n-octyltriethoxysilane under stirring, and then react at 50°C for 24 hours. The product is separated by centrifugation at 12000rpm, washed with methanol, and then vacuum dried (temperature is 50°C, vacuum degree -0.090MPa, unless otherwise specified, other embodiments use the same vacuum drying method) to obtain a solid interfacial solubilizer. At 50°C, take 5g of the above-mentioned solid interfacial solubilizer and add it to 500g of molten stearic acid. Disperse by high-speed shearing. The dispersion time is 20min and the shear rate is 10000rpm to obtain a stearic acid dispersion system. At 50°C, add 20cm 3 Carbon foam (porosity of 80%, pore size of about 10 μm), the system was vacuumed under the temperature condition, the vacuum degree was -0.090 MPa, the treatment time was 24 hours, and after cooling, a carbon foam thermally conductive enhanced phase change composite material was obtained.
[0063] The scanning electron microscope photo of the carbon foam thermal conductive reinforced phase change composite material prepared in this embodiment is as follows: Figure 1 As shown. Figure 1It can be seen that the stearic acid phase change material in this embodiment has been filled into the carbon foam pore structure and has a good filling effect.
[0064] Figure 2 The DSC graph of the carbon foam thermally conductive reinforced phase change composite material prepared in Example 1 of the present invention is shown in FIG. Figure 2 It can be seen that the phase change latent heat of the carbon foam thermal conductive reinforced phase change composite material prepared in this embodiment is 169 J / g.
[0065] The inventors measured the phase change temperature (i.e., the first phase change temperature) of the water-soluble phase change material used, and also measured the phase change temperature (i.e., the second phase change temperature), thermal conductivity, and enthalpy retention rate of the prepared phase change composite material. Other embodiments will use the same method as in Example 1 to measure the same indicators.
[0066] The determination methods of various performance indicators are shown in the following table:
[0067]
[0068] The calculation method of enthalpy retention rate is as follows:
[0069] Enthalpy retention rate = phase change material content = ΔH m / ΔH m0 ×100%;
[0070] Where ΔH m0 is the phase change point enthalpy of the phase change core material, ΔH m is the phase change point enthalpy value of high thermal conductivity phase change material.
[0071] The specific results of the determination are shown in Table 1.
[0072] Example 2
[0073] Weigh 10g of TiO2 nanoparticles with a size of 100nm and add them to 200ml of ethanol. Add 5g of tetrabutyl titanate under stirring, and then react for 6 hours at 30°C. Separate the product by centrifugation at 16000rpm, wash with ethanol, and obtain a solid interface solubilizer by vacuum drying. Under 60°C, take 5g of the above-mentioned solid interface solubilizer and add it to 500g of molten dodecanol, disperse it by high-speed shearing, the dispersion time is 20min, and the shear rate is 10000rpm to obtain an octanoic acid dispersion system. Under 60°C, add 20g of expanded graphite (porosity is 85%, pore size is about 25μm) to the aforementioned octanoic acid dispersion system, vacuumize the system under this temperature condition, the vacuum degree is -0.090MPa, the processing time is 12 hours, and the expanded graphite thermal conductive strengthening phase change composite material is obtained after cooling.
[0074] Example 3
[0075] Weigh 20g of SiO2 nanoparticles with a size of 30nm and add them to 500ml of ethanol. Add 1g of methacryloxypropyltriethoxysilane and 2g of aminopropyltriethoxysilane under stirring, and then react at 70°C for 12 hours. Separate the product by centrifugation at 16000rpm, wash with ethanol, and then obtain a solid interface solubilizer by vacuum drying. At 70°C, take 5g of the above solid interface solubilizer and add it to 500g of molten tetradecanol. Disperse by high-speed shearing. The dispersion time is 20min and the shear rate is 8000rpm to obtain a tetradecanol dispersion system. At 70°C, add 20cm 3 Carbon foam (porosity of 90%, pore size of about 10 μm), the system is vacuumed under the temperature condition, the vacuum degree is -0.090 MPa, the treatment time is 24 hours, and after cooling, a carbon foam thermally conductive reinforced phase change composite material is obtained.
[0076] Example 4
[0077] Weigh 10g of Al2O3 nanoparticles with a size of 15nm and add them to 500ml of ethanol. Add 1g of triisopropyl aluminate under stirring, and then react at 30°C for 36 hours. Separate the product by centrifugation at 20,000rpm, wash with ethanol, and then obtain a solid interface solubilizer by vacuum drying. At 50°C, take 5g of the above solid interface solubilizer and add it to 500g of molten octadecanoic acid. Disperse it by high-speed shearing. The dispersion time is 20min and the shear rate is 10,000rpm to obtain an octadecanoic acid dispersion system. Add 20cm 3 Graphene foam (porosity of 84%, pore size of about 1 μm), the system was vacuumed under the temperature condition, the vacuum degree was -0.080 MPa, the treatment time was 48 hours, and after cooling, the graphene foam thermal conductive reinforced phase change composite material was obtained.
[0078] Example 5
[0079] Weigh 8g of SiO2 nanoparticles with a size of 50nm and add them to 400ml of ethanol. Add 0.5g of phenyltriethoxysilane, 1g of aminopropyltrimethoxysilane and 1g of aminopropyltriethoxysilane under stirring, and then react for 36 hours at 70°C. Separate the product by centrifugation at 16000rpm, wash with ethanol, and obtain a solid interface solubilizer by vacuum drying. At 50°C, take 5g of the above solid interface solubilizer and add it to 500g of molten lauric acid, disperse it by high-speed shearing, the dispersion time is 5min, and the shear rate is 10000rpm to obtain a lauric acid dispersion system. At 50°C, add 150g of carbon nanotubes (porosity is 83% and pore size is about 5μm) to the above-mentioned caprylic acid dispersion system, and pressurize the system under this temperature condition, the pressure is 0.10MPa, the treatment time is 24 hours, and the carbon nanotube thermal conductive enhanced phase change composite material is obtained after cooling.
[0080] Example 6
[0081] Weigh 10g of Al2O3 nanoparticles with a size of 10nm and add them to 500ml of ethanol. Add 3g of triisopropyl aluminate under stirring, and then react at 30°C for 36 hours. Separate the product by centrifugation at 22000rpm, wash with ethanol, and then obtain a solid interface solubilizer by vacuum drying. At 50°C, take 5g of the above solid interface solubilizer and add it to 500g of molten octadecanoic acid. Disperse it by high-speed shearing. The dispersion time is 20min and the shear rate is 10000rpm to obtain an octadecanoic acid dispersion system. Add 20cm 3 Carbon foam (porosity of 85%, pore size of about 10 μm), the system was pressurized under the temperature condition, the pressure was 0.20 MPa, the treatment time was 24 hours, and after cooling, a carbon foam thermally conductive enhanced phase change composite material was obtained.
[0082] Example 7
[0083] Weigh 30g of SiO2 nanoparticles with a size of 200nm and add them to 500mL of ethanol. Add 2g of phenyltriethoxysilane and 1g of aminopropyltrimethoxysilane under stirring, and then react at 40°C for 6 hours. Separate the product by centrifugation at 10,000rpm, wash with ethanol, and then vacuum dry to obtain a solid interface solubilizer. At 140°C, take 5g of the above solid interface solubilizer and add it to 500g of molten erythritol. Disperse it by high-speed shearing. The dispersion time is 10min and the shear rate is 8000rpm to obtain an erythritol dispersion system. At 140°C, add 20cm 3Graphene foam (porosity of 90%, pore size of about 5 μm), under the temperature condition, the system was vacuumed, the vacuum degree was -0.090 MPa, the treatment time was 24 hours, and after cooling, a graphene foam thermally conductive reinforced phase change composite material was obtained.
[0084] Example 8
[0085] Weigh 30g of SnO2 nanoparticles with a size of 200nm and add them to 1000ml of deionized water. Add 5g of tetrabutyl stannate under stirring, and then react at 40°C for 6 hours. Separate the product by centrifugation at 10000rpm, wash with deionized water, and obtain a solid interface solubilizer by vacuum drying. At 140°C, take 5g of the above solid interface solubilizer and add it to 500g of molten erythritol. Disperse it by high-speed shearing. The dispersion time is 10min and the shear rate is 8000rpm to obtain an erythritol dispersion system. Add 20cm 3 Carbon foam (porosity of 85%, pore size of about 15 μm), the system is pressurized under the temperature condition, the pressure is 0.20 MPa, the treatment time is 24 hours, and after cooling, a carbon foam thermally conductive reinforced phase change composite material is obtained.
[0086] Example 9
[0087] The method is substantially the same as that of Example 1, except that sodium dodecylbenzene sulfonate is used instead of the solid interface solubilizer.
[0088] Example 10
[0089] The method is basically the same as that of Example 1, except that Tween-80 is used instead of the solid interface solubilizer.
[0090] Embodiment 11
[0091] The method is substantially the same as that of Example 2, except that OP-10 (polyoxyethylene octylphenol ether-10) is used instead of the solid interface solubilizer.
[0092] Table 1. Properties of the phase change composite materials prepared in various embodiments.
[0093]
[0094] Note: The first phase transition temperature is the phase transition temperature of the water-soluble phase change material used; the second phase transition temperature is the phase transition temperature of the prepared phase change composite material.
[0095] From the results in Table 1, it can be seen that compared with small molecule surfactants, solid interfacial compatibilizers can effectively avoid affecting the performance of the phase change material itself while ensuring a large proportion of the water-soluble phase change material in the porous carbon skeleton, ensuring that the phase change temperature and latent heat of the phase change material are consistent with those before compounding.
[0096] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a phase change composite material, characterized in that: The method comprises the following steps: 1) in a modification solvent, allowing an inorganic reaction precursor and nanoparticles to undergo a modification reaction to achieve surface modification of the nanoparticles, and then separating and drying to obtain a solid interface solubilizer; 2) dispersing the solid interface solubilizing agent in a molten water-soluble phase change material to obtain a phase change material blending system; 3) immersing the carbon-based porous material in the phase change material blending system to obtain a composite impregnation material; 4) Under the condition of vacuum impregnation or pressure infusion, the composite impregnated material is used to realize the compounding of the water-soluble phase change material in the carbon-based porous material to obtain a phase change composite material.
2. The preparation method according to claim 1, characterized in that: The inorganic reaction precursor is selected from at least one of tetra-n-butyl titanate, tetraisopropyl titanate, ethyl orthosilicate, epoxypropyl trimethoxysilane, phenyl triethoxysilane, methacryloxypropyl trimethoxysilane, methacryloxypropyl triethoxysilane, aminopropyl trimethoxysilane, aminopropyl triethoxysilane, phenyl trimethoxysilane, n-octyl triethoxysilane, tetrabutyl stannate, tetrabutyl zirconate, triisopropyl aluminate, and tribenzyl aluminate; and / or The nanoparticles are selected from at least one of aluminum oxide, zirconium oxide, zirconium oxide and titanium oxide; Preferably, the mass ratio of the inorganic reaction precursor to the nanoparticles is 1:0.1-100, preferably 1:1-50.
3. The preparation method according to claim 1 or 2, characterized in that: The carbon-based porous material has a porosity of 70% to 90% and a pore size of 1 μm to 100 μm; The size of the nanoparticles is 1 to 100 nm, more preferably 10 to 50 nm.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The modified solvent is selected from at least one of water, methanol, ethanol, tetrahydrofuran and N,N-dimethylformamide.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The reaction temperature of the modification reaction is 10°C to 70°C, and the reaction time of the modification reaction is 0.5 hours to 72 hours; Preferably, the separation of the solid interface solubilizing agent is carried out by centrifugation, with a centrifugal speed of 3000 to 15000 rpm and a centrifugal time of 2 to 30 minutes.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The water-soluble phase change material is selected from at least one of an alcohol compound and an organic acid compound; Preferably, the alcohol compound is at least one selected from glycerol, tetratetrol, dodecanol, tetradecanol, hexadecanol and erythritol; It is also preferred that the organic acid compound is at least one selected from the group consisting of caprylic acid, capric acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, lauric acid, myristic acid, palmitic acid and stearic acid.
7. The preparation method according to any one of claims 1 to 6, characterized in that In step 2): The dispersion is achieved by high-speed shearing, preferably, the shearing speed of the high-speed shearing is 1000 rpm to 25000 rpm, and the shearing time is 0.5 min to 30 min; or, the dispersion is achieved by ultrasonic treatment, preferably, the ultrasonic treatment frequency of the ultrasonic treatment is 1000 Hz to 40000 Hz, and the ultrasonic treatment time is 10 min to 60 min; In addition, preferably, the dispersing is performed at a temperature 10 to 40° C. higher than the melting point of the water-soluble phase change material.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The carbon-based porous material is selected from at least one of carbon foam, graphene foam, expanded graphite and carbon nanotubes.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The composite process of the phase change material and the carbon-based porous material is achieved by at least one of vacuum impregnation and pressure infusion; Preferably, the compounding is carried out at a temperature 10 to 40° C. higher than the melting point of the water-soluble phase change material; It is further preferred that the vacuum degree of the vacuum impregnation is -0.07MPa to -0.095MPa, more preferably -0.085MPa to -0.090MPa; the treatment time is 1 to 36 hours; In addition, preferably, the pressure of the pressure perfusion is 0.10MPa to -0.30MPa, more preferably 0.15MPa to 0.20MPa; and the treatment time is 1 to 36 hours.
10. A phase change composite material obtained by the preparation method according to any one of claims 1 to 9; Preferably, the thermal conductivity of the phase change composite material is above 20 W / (m·K); and / or The enthalpy value retention rate of the phase change composite material is above 70%.