Inorganic-organic modified ultra-high temperature crosslinking spacer fluid, suspending agent and preparation method thereof
By combining grafting on the surface of inorganic nanoparticles and organic synthetic polymers, cross-linking reaction is formed, the problem of poor temperature resistance performance of the isolation liquid at high temperature is solved, and rheology and suspension stability above 240°C are achieved. Ensure safety of bottom well construction.
Patent Information
- Application Number
- CN202411189411.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing isolation fluid has poor temperature resistance at high temperatures, resulting in solid-phase particle deposition and increased slurry consistency, resulting in failure of channel blockage at the bottom of the well.
Using an inorganic-organic modified ultra-high temperature crosslinking isolation solution, the polymerization of acrylamide or methacrylamide by grafting silane coupling agent on the surface of inorganic nanoparticles, combined with organic synthesis of polymers, and the temperature-resistant monomers are introduced and Adsorbent monomers form cross-linking reaction between amide groups and imine groups, enhancing dispersion and thermal stability.
Under working conditions above 240°C, the isolation liquid has good rheology and suspension stability, and the density difference is less than 0.03g/cm3, which avoids the risk of bottom-hole blockage and pump hold, and ensures construction safety.
Smart Images

Figure CN119081663A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an isolation liquid, in particular to an inorganic-organic modified ultra-high temperature cross-linking isolation liquid, a suspending agent and a preparation method thereof. Background Art
[0002] In recent years, my country has consumed a huge amount of oil resources, and the shallow oil reserves are far from meeting the demand for use. Therefore, the exploration of deep oil resources has become a hot topic. In the deep and ultra-deep wells of oil exploration and development, the isolation fluid is required to have a high density and suitable viscosity, which can not only balance the formation pressure, but also improve the displacement efficiency of the drilling fluid. However, the isolation fluid system currently studied in China generally has poor temperature resistance. Due to the high bottom hole temperature in deep and ultra-deep wells, the Brownian motion of the solid particles in the isolation fluid is aggravated, and the structure of the polymer that provides suspension stress in the isolation fluid is destroyed, causing a large amount of weighted materials in the isolation fluid to sink, resulting in a large difference in density between the upper and lower slurry, affecting construction safety, and even annular blockage, pump choking, and leakage accidents may occur.
[0003] The suspending agents in the currently commonly used isolation fluid system are mainly divided into three categories:
[0004] (1) The first category is inorganic clay mineral materials such as bentonite, sepiolite, attapulgite, and diatomaceous earth. They have special lattice channels. In aqueous solution, water molecules fill the lattice channels, absorb water and swell and disperse in the aqueous solution, forming an "end-end" and "face-end" network structure, converting a large amount of free water into bound water. However, inorganic clay mineral materials themselves have poor temperature resistance. In addition, they have a large specific surface area and a strong ability to adsorb free water. When preparing high-density isolation fluid, the slurry viscosity is relatively high, which makes it difficult to pump the isolation fluid during on-site construction;
[0005] (2) The second category is natural polymer materials such as xanthan gum, sodium carboxymethyl cellulose, hydroxyethyl cellulose, and polyacrylamide. These materials have the advantages of "small amount and high viscosity" and good suspension performance. However, these natural polymers have a common disadvantage: the polymer structure is easily destroyed at high temperatures, the viscosity drops sharply, and the ability to suspend solid particles becomes poor.
[0006] (3) The third category is artificially designed and synthesized polymer materials, which are mainly designed and screened through the functional properties of the required isolation liquid suspension agent to obtain the functional monomers of the synthetic suspension agent, and then prepared by chemical reaction. By introducing hydrophilic groups such as amide, carboxyl, hydroxyl, sulfonic acid, and phosphoric acid groups, such hydrophilic groups can bind free water, increase the viscosity of the solution, and make the polymer material have suspension ability. Secondly, the introduction of benzene rings or other heterocyclic polymerization monomers can improve the temperature resistance of the polymer material. The structure of artificially synthesized polymer materials is flexible and changeable. They can be reasonably designed and prepared according to actual needs. They have stable performance and are currently a popular method for preparing isolation liquid suspension agents. For example, Chinese patent CN202111648639.7 discloses a composite high-temperature resistant flushing isolation liquid suspension agent and its preparation method and application, which can be used for ultra-high temperature (200°C) and high density (2.60g / cm 3 ) working condition, while ensuring the rheological properties, the density can be 2.20~2.60g / cm 3 The free liquid of the isolation liquid at 200℃ is controlled at 0mL, and the density difference after standing for 2h does not exceed 0.030g / cm 3 , effectively improving the sedimentation stability of the high-density isolation liquid system under high temperature and ultra-high temperature conditions.
[0007] However, the number of ultra-deep wells over 8,000 meters in western my country is increasing year by year, and the operating conditions faced by the isolation fluid are more stringent, with formation temperatures generally above 200°C. Under ultra-high temperatures, the conventional isolation fluid system's liquid phase has suspension properties that decompose due to high temperatures, causing solid phase particles to settle. Secondly, the high-density isolation fluid has more solid phase particles, resulting in a thicker isolation fluid slurry. This situation will worsen at high temperatures, and eventually lead to the isolation fluid blocking the channel and cementing failure.
[0008] Therefore, it is necessary to develop an ultra-high temperature cross-linked isolation fluid suitable for working conditions above 200°C to solve the problem of isolation fluid failure under ultra-high temperature and high density. Summary of the invention
[0009] The purpose of the present invention is to provide an inorganic-organic modified ultra-high temperature cross-linking isolation liquid, a suspending agent and a preparation method thereof, which can have good temperature resistance, rheological properties and suspension stability under working conditions above 240°C.
[0010] In order to achieve the above-mentioned object, the present invention provides an inorganic-organic modified ultra-high temperature cross-linked isolation liquid suspension, which comprises the following components in parts by weight: 5 to 8 parts of isolation agent I and 0.1 to 0.15 parts of isolation agent II; wherein the isolation agent II is selected from polyethyleneimine; wherein the isolation agent I is composed of organically modified ultrafine inorganic nanoparticles, organic synthetic high molecular polymers and inorganic clay minerals; the inorganic clay minerals are selected from sepiolite or attapulgite; the organically modified ultrafine inorganic nanoparticles are obtained by The surface-grafted silane coupling agent is polymerized with acrylamide or methacrylamide via an initiator in an inert gas atmosphere to obtain the obtained product; the organic synthetic high molecular polymer is obtained by polymerizing an adsorptive monomer with a temperature-sensitive monomer and a temperature-resistant monomer via an initiator in an inert gas atmosphere; wherein the adsorptive monomer is selected from acrylamide or methacrylamide; the temperature-sensitive monomer is selected from N,N-dimethylacrylamide or N,N-diethylacrylamide; the temperature-resistant monomer is selected from sodium p-styrene sulfonate, N-vinyl pyrrolidone or N-vinyl caprolactam.
[0011] The ultrafine nanoparticles used in the present invention have a large specific surface area and strong surface activity. The active hydroxyl groups on the surface of the ultrafine nanoparticles can undergo dehydration condensation with the silanol groups of the chemical reagent silane coupling agent in the aqueous solution, so that the ultrafine nanoparticles have enhanced dispersibility. The surface is connected with carbon-carbon double bonds, which is convenient for subsequent polymerization reactions, thereby changing the chemical properties of the ultrafine nanoparticles. By grafting a monomer with an amide group on the surface of the nanoparticles, the dispersibility of the nanoparticles in organic solutions is enhanced, and reactive groups are provided for subsequent cross-linking with organic synthetic high molecular polymers. In addition, the nanoparticles used in the present invention not only have higher thermal stability, but also can react with alkaline substances in the cement slurry to generate silicates when being subsequently replaced by cement slurry, thereby improving the interface cement strength.
[0012] The inorganic clay minerals of the present invention are sepiolite and attapulgite, which have good thermal stability.
[0013] The organic synthetic high molecular polymer of the present invention is prepared by free radical polymerization reaction by introducing a heat-resistant monomer, an adsorptive monomer (with an amide group) and a temperature-sensitive monomer as polymerization monomers of the organic synthetic high molecular polymer. These monomers are selected according to the required performance of the isolation liquid at high temperature, wherein the adsorptive monomer mainly provides liquid phase viscosity and enhances the suspension of the polymer; the temperature-sensitive monomer prevents the viscosity from dropping sharply at high temperature, enables the polymer to produce hydrophobic association characteristics at high temperature, and slows down the trend of the polymer viscosity decreasing at high temperature; the heat-resistant monomer directly improves the thermal stability of the suspension agent at high temperature and enhances the rigidity of the polymer molecular chain. The present invention adopts inorganic clay minerals, most of which are "layered" and "needle-shaped" in structure. They have special lattice channels, absorb water and swell, are dispersed in aqueous solution, bind free water, and increase viscosity.
[0014] In the components of the present invention, at 200° C., the amide groups in the organically modified ultrafine inorganic nanoparticles and the amide groups in the organic synthetic high molecular polymer will respectively undergo cross-linking reactions with the imine groups in the isolation agent II.
[0015] Preferably, the mass ratio of the organically modified ultrafine inorganic nanoparticles, the organic synthetic high polymer and the inorganic clay mineral is 1:2 to 3:1.
[0016] Preferably, the molecular weight of the polyethyleneimine is 3 million to 7 million.
[0017] Preferably, the inorganic nanoparticles are selected from nano-silicon dioxide or nano-aluminum oxide to enhance the temperature resistance of the polymer at high temperatures.
[0018] Preferably, in the organically modified ultrafine inorganic nanoparticles, the mass ratio of the silane coupling agent to the inorganic nanoparticles is (3-5):100; the mass ratio of the inorganic nanoparticles with the surface grafted silane coupling agent to acrylamide or methacrylamide is (10-20):(1-2).
[0019] Preferably, in the organic synthetic high molecular polymer, the mass ratio of the adsorptive monomer to the temperature-sensitive monomer and the temperature-resistant monomer is (74-89): (12-25): (17-36).
[0020] Preferably, the initiator is selected from ammonium persulfate or potassium persulfate; or / and the silane coupling agent is selected from silane coupling agent KH550 (γ-aminopropyltriethoxysilane) and KH570 (γ-methacryloxypropyltrimethoxysilane); or / and the inorganic nanoparticles are selected from nano-silicon dioxide or nano-aluminum oxide, and the inorganic nanoparticles can enhance the temperature resistance of the polymer at high temperatures.
[0021] Preferably, in the organically modified ultrafine inorganic nanoparticles, the mass ratio of the initiator to acrylamide or methacrylamide is (0.033-0.066):(1-2); in the organic synthetic high molecular polymer, the mass ratio of the total mass of the adsorptive monomer, the temperature-sensitive monomer and the temperature-resistant monomer to the initiator is (125-137):0.37.
[0022] Another object of the present invention is to provide an ultra-high temperature cross-linked isolation liquid containing the suspending agent.
[0023] Preferably, the isolation liquid is composed of the following components in parts by weight: 5 to 8 parts of isolation agent I, 0.1 to 0.15 parts of isolation agent II, 2 to 3 parts of surfactant, 0.3 parts of defoamer, 140 to 272 parts of density regulator and 100 parts of water. Controlling each component within this range can ensure that the isolation liquid has good rheology and suspension stability. The present invention needs to control the amount of isolation liquid I and isolation agent II in the suspension agent. If the amount added exceeds the above range, the isolation liquid slurry will be too thick and the rheology will deteriorate. If the amount added is less than the above range, the suspension stability of the isolation liquid will deteriorate at high temperatures.
[0024] Preferably, the surfactant is selected from cationic surfactants, and the cationic surfactant is selected from octadecyltrimethylammonium bromide or octadecyldimethylbenzylammonium chloride; the defoaming agent is selected from tributyl phosphate; and the density regulator is selected from barite and / or iron ore powder.
[0025] Preferably, the density is less than 2.30 g / cm 3 The isolation liquid system uses barite as the density regulator; the density is 2.30g / cm 3 The isolation liquid system, the density regulator is selected from barite: iron ore powder in a mass ratio of (9-7): (1-3).
[0026] More preferably, the density is 2.30 g / cm 3 The isolation liquid system uses a density regulator with a mass ratio of 9:1 barite: iron ore powder. Too large a proportion of iron ore powder will affect the suspension stability of the isolation liquid.
[0027] The surfactant used in the present invention is a cationic surfactant, which utilizes its positively charged parts to attract negatively charged inorganic clay minerals through electrostatic attraction to disperse them in the polymer solution, thereby preventing the inorganic clay minerals from agglomerating and settling in the organic solvent.
[0028] Another object of the present invention is to provide a method for preparing the suspension concentrate, the method comprising:
[0029] The preparation of the organically modified ultrafine inorganic nanoparticles comprises:
[0030] (S1) placing inorganic nanoparticles and a silane coupling agent in water and adjusting the pH value to 6 to 7;
[0031] (S2) heating and stirring the reaction;
[0032] (S3) After the reaction is completed, cooling to room temperature, centrifuging, washing, filtering, drying, and grinding to obtain inorganic nanoparticles with surface modification and silane coupling agent;
[0033] (S4) placing a reaction monomer in water, wherein the reaction monomer is the inorganic nanoparticles with surface-modified silane coupling agents and acrylamide or methacrylamide, adjusting the pH value to 6-7, and adjusting the reaction monomer concentration to 11%-19%;
[0034] (S5) heating and stirring the reaction under an inert gas atmosphere, and dropping an initiator to polymerize the mixture;
[0035] (S6) After the reaction is completed, cooling to room temperature, centrifuging, washing, filtering, and drying to obtain the organically modified ultrafine inorganic nanoparticles;
[0036] The preparation of the organic synthetic high molecular polymer comprises:
[0037] (S10) placing the adsorptive monomer, the thermosensitive monomer and the thermoresistant monomer in water and adjusting the pH value to 6 to 7;
[0038] (S20) heating and stirring the reaction under an inert gas atmosphere, and dropping an initiator to polymerize the mixture;
[0039] (S30) After the reaction is completed, freeze-drying and grinding into powder to obtain an organic synthetic high molecular polymer.
[0040] Preferably, in steps (S2), (S5) and (S20), the heating temperature is 50 to 60°C.
[0041] Preferably, the dropping speed of the initiator is 1 mL / min.
[0042] Preferably, in step (S2), the stirring speed is 800-1200 r / min; and in steps (S5) and (S20), the stirring speed is 200-300 r / min.
[0043] Preferably, the inert gas is nitrogen (N2) or argon (Ar).
[0044] The preparation of the inorganic-organic modified ultra-high temperature cross-linked isolation liquid of the present invention comprises: firstly adding isolation agent I into water, and after the isolation agent I is completely dissolved, adding surfactant and defoaming agent, mixing evenly, and finally adding isolation agent II to obtain isolation liquid base liquid; adding density regulator into the isolation liquid base liquid to form the final ultra-high temperature cross-linked isolation liquid.
[0045] The inorganic-organic modified ultra-high temperature cross-linked isolation fluid, suspension agent and preparation method thereof of the present invention solve the problem of the isolation fluid failing to work at a high temperature above 200° C. and have the following advantages:
[0046] In the release agent I of the present invention, the organically modified ultrafine nanoparticles are introduced with unsaturated bonds, i.e., carbon-carbon double bonds, on the surface of the ultrafine nanoparticles by adding a silane coupling agent, and on this basis, a free radical polymerization reaction occurs with a polymer monomer with an amide group, and an amide group is introduced on its surface, thereby enhancing the dispersibility of the ultrafine nanoparticles in the polymer and providing a reactive group for the subsequent use of the release agent II (PEI); in the composition structure of the organic synthetic high molecular polymer material, the temperature-resistant monomer provides a heterocyclic or benzene ring rigid group to improve the thermal stability of the polymer, the adsorbent monomer provides suspension performance, and the temperature-sensitive monomer makes the polymer have the characteristic of hydrophobic association to alleviate the trend of the polymer viscosity decreasing at high temperature in the aqueous solution. Release agent II (PEI) is a connecting bridge between the organically modified ultrafine nanoparticles and the organic synthetic high molecular polymer material, and the amide groups in the two materials and the imine groups in PEI undergo an electrophilic substitution reaction at high temperature, so that the two are respectively cross-linked through the PEI molecule to form NN covalent bonds, forming a more stable and more complex inorganic-organic hybrid three-dimensional network structure.
[0047] The inorganic-organic modified ultra-high temperature cross-linked isolation liquid of the present invention can be applied to 240°C, and the adjustable density is 1.80-2.30 g / cm 3 The formation environment has good sedimentation stability at high temperature, and the density difference between the upper and lower parts is less than 0.03g / cm 3 The settlement thickness is 0 cm and the invention has good rheological properties. The invention effectively alleviates the instability of the spacer fluid weighting agent at high temperature at the bottom of a deep well or ultra-deep well, and has a significant impact on ensuring the safety of cementing work. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is the Fourier infrared spectrum of the organically modified ultrafine nanoparticles prepared in Example 3 of the present invention.
[0049] Figure 2 This is the Fourier infrared spectrum of the organic synthetic high molecular polymer material prepared in Example 3 of the present invention.
[0050] Figure 3Schematic diagram of the stability in water of the physical mixed material of unmodified ultrafine nanoparticles and organic synthetic high polymer and the physical mixed material of organically modified ultrafine inorganic nanoparticles and organic synthetic high polymer in Example 3 of the present invention.
[0051] Figure 4 The thermogravimetric spectra of the physical mixed material of organically modified ultrafine inorganic nanoparticles and organic synthetic high molecular polymer prepared in Example 3 of the present invention in isolation agent II at different temperatures. DETAILED DESCRIPTION
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] An inorganic-organic modified ultra-high temperature cross-linked isolation fluid, which is composed of the following components in parts by weight: 5 parts of isolation agent I, 0.15 parts of isolation agent II, 2 parts of surfactant (octadecyl trimethyl ammonium bromide), 0.3 parts of defoaming agent (tributyl phosphate), 140 parts of density regulator (baryte) and 100 parts of water. The density of the ultra-high temperature cross-linked isolation fluid is 1.80 g / cm 3 , recorded as isolation fluid A.
[0055] Among them, the isolation agent I is composed of organically modified ultrafine inorganic nanoparticles, organic synthetic high molecular polymers and sepiolite, and the mass ratio of organically modified ultrafine inorganic nanoparticles, organic synthetic high molecular polymers and sepiolite is 1:2:1. The isolation agent II is polyethyleneimine (PEI) with a molecular weight of 3 million to 7 million (purchased from Shanghai MacLean Biochemical Technology Co., Ltd.). The isolation agent I and the isolation agent II are used as suspending agents.
[0056] The preparation method of the above organically modified ultrafine inorganic nanoparticles, the raw materials are calculated by weight, as follows:
[0057] (S1) dissolving 15 parts of nano-silica particles and 3% (based on the mass of the nano-silica particles) of silane coupling agent KH550 in 100 parts of deionized water, and adjusting the pH value to 6 with sodium hydroxide solution;
[0058] (S2) transferring the mixed solution obtained in step (S1) into a three-necked flask, setting the stirring speed to 800 r / min, the temperature to 50° C., and reacting for 4 h;
[0059] (S3) After the reaction is completed, the mixture is cooled to room temperature, the mixture is centrifuged at high speed, washed with deionized water, filtered, dried, and ground to obtain surface-modified nano-silicon dioxide particles with a silane coupling agent;
[0060] (S4) dissolving 10 parts of the surface-modified nano-silica particles with a silane coupling agent and 1 part of acrylamide in 70 parts of deionized water, adjusting the pH value to 6 with a sodium hydroxide solution, and then adding deionized water to adjust the mass percentage concentration of the reaction monomers (the surface-modified nano-silica particles with a silane coupling agent and acrylamide) to 11.1%;
[0061] (S5) transferring the mixed solution obtained in step (S4) to a three-necked flask, setting the stirring speed to 200 r / min, the temperature to 50° C., introducing nitrogen for 10 min, and adding the initiator dropwise at a rate of 1 mL / min for 10 min using a syringe. After the addition of the initiator is completed, react for 4 h; wherein the initiator is prepared by dissolving 0.033 parts of ammonium persulfate in 10 parts of deionized water;
[0062] (S6) After the reaction is completed, the mixture is cooled to room temperature, centrifuged at high speed, washed with deionized water, filtered, and dried to obtain organically modified ultrafine inorganic nanoparticles.
[0063] The preparation method of the above organic synthetic high molecular polymer, the raw materials are calculated by weight, as follows:
[0064] (S10) dissolving 88.18 parts of acrylamide monomer in 490 parts of deionized water, adding 35.56 parts of sodium p-styrene sulfonate and 12.82 parts of N,N-dimethylacrylamide, and adjusting the pH value to 6 with sodium hydroxide solution;
[0065] (S20) transferring the mixed solution obtained in step (S10) to a three-necked flask, setting the stirring speed to 200 r / min, the temperature to 50° C., introducing nitrogen for 10 min, and adding the initiator dropwise at a rate of 1 mL / min for 10 min using a syringe. After the initiator is added dropwise, react for 4 h; wherein the initiator is prepared by dissolving 0.37 parts of ammonium persulfate in 10 parts of deionized water;
[0066] (S30) After the reaction is completed, a colorless, transparent, viscous solution is obtained, which is freeze-dried and ground into powder, namely, an organic synthetic high molecular polymer.
[0067] The preparation of the inorganic-organic modified ultra-high temperature cross-linked isolation liquid of this embodiment is as follows:
[0068] First, add the isolation agent I into the water. After the isolation agent I is completely dissolved, add the surfactant (octadecyl trimethyl ammonium bromide) and the defoaming agent (tributyl phosphate). After mixing evenly, add the isolation agent II to obtain the isolation liquid base liquid. Add the density regulator to the isolation liquid base liquid to form the final ultra-high temperature cross-linking isolation liquid.
[0069] Example 2
[0070] An inorganic-organic modified ultra-high temperature cross-linked isolation fluid, which is composed of the following components in parts by weight: 8 parts of isolation agent I, 0.1 parts of isolation agent II, 3 parts of surfactant (octadecyl trimethyl ammonium bromide), 0.3 parts of defoaming agent (tributyl phosphate), 190 parts of density regulator (baryte) and 100 parts of water. The density of the ultra-high temperature cross-linked isolation fluid is 2.00 g / cm 3 , recorded as isolation fluid B.
[0071] The release agent I is composed of organically modified ultrafine inorganic nanoparticles, organic synthetic high polymers and attapulgite, and the mass ratio of the organically modified ultrafine inorganic nanoparticles, organic synthetic high polymers and attapulgite is 1:3:1. The release agent II is the same as that of Example 1.
[0072] The preparation method of the above organically modified ultrafine inorganic nanoparticles, the raw materials are calculated by weight, as follows:
[0073] (S1) dissolving 25 parts of nano-aluminum oxide particles and 5% (based on the mass of the nano-aluminum oxide particles) of silane coupling agent KH570 in 100 parts of deionized water, and adjusting the pH value to 6 with sodium bicarbonate solution;
[0074] (S2) is the same as step (S2) of Example 1;
[0075] (S3) After the reaction is completed, the mixture is cooled to room temperature, the mixture is centrifuged at high speed, washed with deionized water, filtered, dried, and ground to obtain surface-modified nano-aluminum oxide particles with a silane coupling agent;
[0076] (S4) dissolving 20 parts of the surface-modified nano-aluminum oxide particles with a silane coupling agent and 2 parts of acrylamide in 70 parts of deionized water, adjusting the pH value to 6 with a sodium hydroxide solution, and adding deionized water to adjust the monomer (surface-modified nano-aluminum oxide particles with a silane coupling agent and acrylamide) mass percentage concentration of the reaction solution to 18.03%;
[0077] (S5) is the same as step (S5) of Example 1, except that the initiator is prepared by dissolving 0.066 parts of ammonium persulfate in 10 parts of deionized water;
[0078] (S6) The same as step (S5) of Example 1, to obtain the organically modified nano-aluminum oxide particles of this example.
[0079] The preparation method of the above organic synthetic high molecular polymer, the raw materials are calculated by weight, as follows:
[0080] (S10) dissolving 82.90 parts of methacrylamide monomer in 490 parts of deionized water, adding 17.32 parts of N-vinyl pyrrolidone and 24.78 parts of N,N-diethylacrylamide, and adjusting the pH value to 6 with sodium bicarbonate solution;
[0081] (S20) is the same as step (S20) of Example 1;
[0082] (S30) The same as step (S30) of Example 1 is performed to obtain the organic synthetic high molecular polymer of this example.
[0083] Example 3
[0084] An inorganic-organic modified ultra-high temperature cross-linked isolation fluid, which is composed of the following components in parts by weight: 6 parts of isolation agent I, 0.1 parts of isolation agent II, 3 parts of surfactant (octadecyl trimethyl ammonium bromide), 0.3 parts of defoaming agent (tributyl phosphate), 272 parts of density regulator (the mass ratio of barite to iron ore powder is 9:1) and 100 parts of water. The density of the ultra-high temperature cross-linked isolation fluid is 2.30 g / cm 3 , recorded as isolation fluid C.
[0085] The release agent I is composed of organically modified ultrafine inorganic nanoparticles, organic synthetic high polymers and sepiolite, and the mass ratio of the organically modified ultrafine inorganic nanoparticles, organic synthetic high polymers and sepiolite is 1:2.7:1. The release agent II is the same as that of Example 1.
[0086] The preparation method of the above organically modified ultrafine inorganic nanoparticles, the raw materials are calculated by weight, as follows:
[0087] (S1) dissolving 15 parts of nano-silica particles and 5% (based on the mass of the nano-silica particles) of silane coupling agent KH570 in 100 parts of deionized water, and adjusting the pH value to 6 with sodium hydroxide solution;
[0088] (S2) is the same as step (S2) of Example 1;
[0089] (S3) After the reaction is completed, the mixture is cooled to room temperature, the mixture is centrifuged at high speed, washed with deionized water, filtered, dried, and ground to obtain surface-modified nano-silicon dioxide particles with a silane coupling agent;
[0090] (S4) dissolving 10 parts of the surface-modified nano-silica particles with silane coupling agents and 1 part of methacrylamide in 70 parts of deionized water, adjusting the pH value to 6 with sodium hydroxide solution, and adding deionized water to adjust the mass percentage concentration of the monomers (surface-modified nano-silica particles with silane coupling agents and methacrylamide) in the reaction solution to 11.1%;
[0091] (S5) is the same as step (S5) of Example 1, except that the initiator is prepared by dissolving 0.033 parts of potassium persulfate in 10 parts of deionized water;
[0092] (S6) The same as step (S5) of Example 1, to obtain the organically modified nano-aluminum oxide particles of this example.
[0093] The preparation method of the above organic synthetic high molecular polymer material is as follows:
[0094] (S10) dissolving 81.80 parts of acrylamide monomer in 490 parts of deionized water, adding 25.63 parts of N-vinyl caprolactam and 17.56 parts of N,N-diethylacrylamide, and adjusting the pH value to 6 with sodium hydroxide solution;
[0095] (S20) is the same as step (S20) of Example 1, except that: the initiator is prepared by dissolving 0.37 parts of potassium persulfate in 10 parts of deionized water;
[0096] (S30) The same as step (S30) of Example 1 is performed to obtain the organic synthetic high molecular polymer of this example.
[0097] Comparative Example 1
[0098] An inorganic-organic modified cross-linked spacer liquid, whose components and contents are substantially the same as those in Example 1, except that no spacer II is added, and the density of the cross-linked spacer liquid is 1.80 g / cm 3 , recorded as isolation fluid D.
[0099] Experimental Example 1 Performance Test
[0100] The above-mentioned isolation liquids A to D were respectively placed in a high-temperature heating roller furnace for heating for 5 hours at 240°C, and then placed in a 90°C water bath for 2 hours. The performance of each isolation liquid was evaluated as follows.
[0101] 1. Test the sedimentation stability of the isolation liquid at 240℃
[0102] The isolation liquid system was subjected to a 240°C sedimentation stability test, and the performance results are shown in Table 1 below.
[0103] Table 1 Test results of the settling stability performance of the isolation fluid
[0104]
[0105] 2. Test the rheological properties of the isolation fluid at 240°C
[0106] The rheological properties of the isolation liquid system were tested at 240°C, and the performance results are shown in Table 2 below.
[0107] Table 2 Rheological properties test results of the isolation fluid
[0108]
[0109] Note: The rheological parameters at 240℃ were measured by a six-speed rotary viscometer. The following readings.
[0110] It can be seen from Tables 1 and 2 that the inorganic-organic modified ultra-high temperature cross-linked isolation fluids A to C under 240°C high temperature hot rolling curing have good sedimentation stability and rheological properties, with fluidity between 20 and 23 cm, and no free liquid is generated; through test data calculation, it can be obtained that after 240°C high temperature treatment, the upper and lower density differences of the isolation fluids A to C are all less than 0.03 g / cm 3 .
[0111] By comparing the isolation liquid A and the isolation liquid D, the density difference of the isolation liquid D without the effect of isolation agent II is 0.13g / cm 3 , the deposition thickness is 0.4cm, the organically modified ultrafine inorganic nanoparticles and organic synthetic polymers play their own roles, and both have a certain viscosity reduction at high temperatures. For the isolation liquid A, the electrophilic substitution reaction between polyethyleneimine (PEI) and amide group (-NH2) at high temperature is used to generate chemical crosslinking in the form of NN covalent bonds to form a more stable network skeleton support weighting agent for the organically modified ultrafine inorganic nanoparticles and organic synthetic polymers in aqueous solution. While PEI connects the two materials at high temperatures, it can also make the original three-dimensional network structure more complicated, thereby improving the thermal stability of the isolation liquid.
[0112] 3. Temperature resistance of organic synthetic polymer components of isolation fluid
[0113] Three groups of materials were set up, namely water, a physical mixture of unmodified ultrafine nanoparticles and organic synthetic polymers in Example 3, and a physical mixture of organically modified ultrafine inorganic nanoparticles and organic synthetic polymers prepared in Example 3. They were respectively loaded into 50 mL sedimentation tubes and the experimental phenomena were observed after standing for 1 day.
[0114] like Figure 3As shown in the figure, (A) is water, (B) is the physical mixed material of the unmodified ultrafine nanoparticles and the organic synthetic high molecular polymer in Example 3, and (C) is the physical mixed material of the organically modified ultrafine inorganic nanoparticles and the organic synthetic high molecular polymer prepared in Example 3. It can be observed from the figure that simply blending nanosilica with polymer will cause the nanosilica to agglomerate. The modified nanosilica can be grafted into the polymer system to form an inorganic-organic hybrid structure and has good dispersibility.
[0115] like Figure 4 As shown in the figure, it can be observed that as the temperature increases, the decomposition temperature of the mixed material increases, the reaction rate of the isolation liquid and the cross-linking agent accelerates, and after the degree of cross-linking increases, the thermal stability of the isolation liquid is improved, the decomposition temperature increases, and the temperature resistance is enhanced.
[0116] In summary, the adjustable range of the isolation liquid system density is 1.80~2.30g / cm 3 , and under curing at a temperature of 240°C, they all have good rheological properties and sedimentation stability, which further proves that the inorganic-organic modified ultra-high temperature cross-linked isolation fluid of the present invention has high temperature resistance, so that during the entire cementing process, there will be no serious risk of weighting agent sedimentation, annulus blockage, and pump suffocation, thereby ensuring the smooth progress of the construction process.
[0117] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. An inorganic-organic modified ultra-high temperature cross-linked spacer liquid suspending agent, characterized in that: The suspending agent comprises the following components in parts by weight: 5 to 8 parts of an isolating agent I and 0.1 to 0.15 parts of an isolating agent II; wherein the isolating agent II is selected from polyethylene imine; Wherein, the isolation agent I is composed of organically modified ultrafine inorganic nanoparticles, organic synthetic high molecular polymers and inorganic clay minerals; the inorganic clay minerals are selected from sepiolite or attapulgite; The organically modified ultrafine inorganic nanoparticles are obtained by grafting a silane coupling agent on the surface of the inorganic nanoparticles and then polymerizing with acrylamide or methacrylamide via an initiator in an inert gas atmosphere; The organic synthetic high molecular polymer is obtained by polymerizing an adsorptive monomer, a temperature-sensitive monomer and a temperature-resistant monomer under an inert gas atmosphere via an initiator; wherein the adsorptive monomer is selected from acrylamide or methacrylamide; the temperature-sensitive monomer is selected from N,N-dimethylacrylamide or N,N-diethylacrylamide; and the temperature-resistant monomer is selected from sodium p-styrene sulfonate, N-vinyl pyrrolidone or N-vinyl caprolactam.
2. The suspending agent according to claim 1, characterized in that The mass ratio of the organically modified ultrafine inorganic nanoparticles, the organic synthetic high molecular polymer and the inorganic clay mineral is 1:2-3:
1.
3. The suspending agent according to claim 1, characterized in that In the organically modified ultrafine inorganic nanoparticles, the mass ratio of the silane coupling agent to the inorganic nanoparticles is (3-5):100; the mass ratio of the inorganic nanoparticles with the surface grafted silane coupling agent to acrylamide or methacrylamide is (10-20):(1-2).
4. The suspending agent according to claim 1, characterized in that In the organic synthetic high molecular polymer, the mass ratio of the adsorptive monomer to the temperature-sensitive monomer and the temperature-resistant monomer is (74-89): (12~25):(17~36)。 5. The suspension concentrate according to any one of claims 1 to 4, characterized in that The initiator is selected from ammonium persulfate or potassium persulfate; or / and The silane coupling agent is selected from silane coupling agent KH550, KH570; or / and The inorganic nanoparticles are selected from nano silicon dioxide or nano aluminum oxide.
6. An ultra-high temperature cross-linked isolation liquid containing the suspending agent according to any one of claims 1 to 5.
7. The isolation liquid according to claim 6, characterized in that: The isolation liquid is composed of the following components in parts by weight: 5 to 8 parts of isolation agent I, 0.1 to 0.15 parts of isolation agent II, 2 to 3 parts of surfactant, 0.3 parts of defoaming agent, 140 to 272 parts of density regulator and 100 parts of water.
8. The isolation liquid according to claim 7, characterized in that: The surfactant is selected from cationic surfactants, and the cationic surfactant is selected from octadecyltrimethylammonium bromide or octadecyldimethylbenzylammonium chloride; the defoamer is selected from tributyl phosphate; and the density regulator is selected from barite and / or iron ore powder.
9. The method for preparing a suspension concentrate according to claim 1, wherein The method includes: The preparation of the organically modified ultrafine inorganic nanoparticles comprises: (S1) placing inorganic nanoparticles and a silane coupling agent in water and adjusting the pH value to 6 to 7; (S2) heating and stirring the reaction; (S3) After the reaction is completed, cooling to room temperature, centrifuging, washing, filtering, drying, and grinding to obtain surface-modified inorganic nanoparticles with a silane coupling agent; (S4) placing a reaction monomer in water, wherein the reaction monomer is the inorganic nanoparticles with surface-modified silane coupling agents and acrylamide or methacrylamide, adjusting the pH value to 6 to 7, and adjusting the reaction monomer concentration to 11% to 19%; (S5) heating and stirring the reaction under an inert gas atmosphere, and dropping an initiator to polymerize the mixture; (S6) After the reaction is completed, cooling to room temperature, centrifuging, washing, filtering, and drying to obtain the organically modified ultrafine inorganic nanoparticles; The preparation of the organic synthetic high molecular polymer comprises: (S10) placing the adsorptive monomer, the thermosensitive monomer and the thermoresistant monomer in water and adjusting the pH value to 6 to 7; (S20) heating and stirring the reaction under an inert gas atmosphere, and dropping an initiator to polymerize the mixture; (S30) After the reaction is completed, freeze-drying and grinding into powder to obtain an organic synthetic high molecular polymer.
10. The preparation method according to claim 9, characterized in that: In steps (S2), (S5), and (S20), the heating temperature is 50 to 60°C.