Rare earth doped fluoride nanocrystal surface structure reconstruction method
The cationic vacancy on the surface of the nanocrystals is filled by wet chemical treatment, and the lattice defects of rare earth-doped fluoride nanocrystals are eliminated, and the problem of degradation of nanocrystal luminescence performance is solved, high luminescence efficiency and stability are achieved, process is simplified, and process is expanded. Applications in the biological field.
Patent Information
- Application Number
- CN202411188531.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The surface lattice defect of rare earth-doped fluoride nanocrystals leads to a degradation of luminescence performance. The existing methods are difficult to effectively eliminate defects and have complex processes, which limits its application in the biological field.
Through wet chemical treatment, inert rare earth ions are used to fill the cationic vacancy on the surface of the nanocrystals to eliminate lattice defects. A mixed solution of oleic acid and 1-octene is used as solvent to prepare the precursor solution and the initial rare earth doped fluoride nanometers The cyclohexane dispersion of the crystal is mixed, the temperature and centrifugal washing conditions are controlled, and the surface structure reconstruction of rare earth-doped fluoride nanocrystals is realized.
Its luminous efficiency and stability are significantly enhanced without changing the size of nanocrystals, simplifying the process, ease of mass production, and expanding its application possibilities in bioimaging and other fields.
Smart Images

Figure CN119081696A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for reconstructing the surface structure of a nanocrystal, and belongs to the field of rare earth doped fluoride luminescent nanocrystals. Background Art
[0002] Rare earth-doped fluoride nanocrystals have important applications in bioimaging, biosensing, photovoltaic devices, and photochemical reactions due to their unique physical and chemical properties, such as long-lived emission, narrow bandwidth, high resistance to photo-scintillation, and strong resistance to photo-bleaching.
[0003] Among them, the biological field has special requirements for rare earth doped fluoride nanocrystals with small size and high luminescence intensity. However, the presence of lattice defects on the surface of nanocrystals seriously reduces their luminescence performance. In particular, as the size of rare earth doped fluoride nanocrystals decreases, the quenching effect caused by their surface lattice defects becomes stronger, making it difficult to meet the demand for high luminescence brightness, which greatly limits the application of rare earth doped fluoride nanocrystals in the biological field.
[0004] At present, researchers mainly try to solve this problem by constructing core-shell structures, dye sensitization, surface plasmon coupling, dielectric microlens modulation and photonic crystal engineering, but these methods have their own limitations. For example, the construction of core-shell structures is often accompanied by the increase in the size of rare earth-doped fluoride nanocrystals, while the other methods have the disadvantages of cumbersome operation and complex process. More importantly, the above methods have failed to fundamentally eliminate the lattice defects on the crystal surface, and the actual effect is limited. Summary of the invention
[0005] The present invention aims to solve the technical problems that the existing method of eliminating lattice defects on the surface of nanocrystals will increase the crystal size and the process is complicated, and to provide a method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals. By adopting a simple preparation process, the rare earth-doped fluoride nanocrystals can achieve the effect of both meeting the small size requirement and having high luminous intensity without changing the crystal size.
[0006] The method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals of the present invention is carried out according to the following steps:
[0007] 1. A precursor solution is prepared by using a mixed solution of oleic acid and 1-octadecene as a solvent and a soluble salt of an inert rare earth ion as a solute; wherein the inert rare earth ion is yttrium (Y), lutetium (Lu), gadolinium (Gd) or lanthanum (La);
[0008] 2. Mixing the initial rare earth doped fluoride nanocrystal cyclohexane dispersion with the precursor solution, wherein the ratio of the amount of trivalent cations in the initial rare earth doped fluoride nanocrystal cyclohexane dispersion to the amount of rare earth ions in the precursor solution is 1:(1-8); then, keeping the mixture at a temperature of 100-180°C for 10-30 minutes to remove cyclohexane and water in the mixture, then heating it to 200-300°C and keeping it for 5-90 minutes, then cooling it to room temperature, pouring the resulting liquid into a centrifuge tube, adding ethanol, and centrifuging and washing it at a speed of 5000-10000 r / min for 5-15 minutes; after repeating the centrifugal washing 2-3 times, dispersing it in cyclohexane to complete the surface structure reconstruction of the rare earth doped fluoride nanocrystals.
[0009] Furthermore, the size of the rare earth-doped fluoride nanocrystals in the initial cyclohexane dispersion of the rare earth-doped fluoride nanocrystals is 5 to 60 nm.
[0010] Furthermore, in the mixed solution of oleic acid and 1-octadecene described in step 1, the volume ratio of oleic acid to 1-octadecene is 1:(1-3).
[0011] Furthermore, the precursor solution in step 1 contains 0.5-4 mmol of inert rare earth ions per 10 ml of the precursor solution.
[0012] Furthermore, the soluble salt of the inert rare earth ion in step 1 is an acetate or chloride salt of the inert rare earth ion.
[0013] Furthermore, the preparation method of the precursor solution described in step one is as follows: a soluble salt of an inert rare earth ion is added to a mixed solution of oleic acid and 1-octadecene, and under the protection of an inert gas such as nitrogen or argon, the mixture is stirred and heated to 100-160° C. and maintained for 10-60 minutes to fully dissolve the raw materials to obtain a precursor solution.
[0014] Furthermore, the initial rare earth-doped fluoride nanocrystals in step 2 are, for example, LiYF4, LiLuF4, LiGdF4, NaYF4 or NaGdF4.
[0015] The method for reconstructing the surface structure of rare earth doped fluoride nanocrystals of the present invention uses inert rare earth ions (such as Y / Lu / Gd / La, etc.) to fill the cation vacancies on the surface of the nanocrystals through a wet chemical treatment method, thereby eliminating the surface lattice defects and achieving the enhancement of rare earth ion luminescence without changing the size of the rare earth doped fluoride nanocrystals.
[0016] Advantages of the present invention: 1. The present invention eliminates lattice defects on the surface of rare earth-doped fluoride nanocrystals without changing the size of the rare earth-doped fluoride nanocrystals, significantly enhancing the luminescence efficiency and stability of rare earth-doped fluoride nanocrystals. This discovery has opened up a new path for the optimization of nanomaterials and their applications in ultra-high resolution imaging and biological fields. 2. The surface structure reconstruction operation process is relatively simple, requiring only changes in reaction conditions (such as the ratio of nanocrystals to rare earth ion precursors, temperature, reaction time, etc.), without the need for complex chemical modifications or new synthesis steps. Therefore, it is easy to mass produce and put into practical use. This method is not only of great significance for improving the luminescence properties of various nanocrystals, but also provides new possibilities for expanding their applications in biological imaging and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a transmission electron microscope photograph of LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 of Example 1;
[0018] Figure 2 is a transmission electron microscope photograph of LiYF4:25%Yb,0.5%Tm nanocrystals after surface structure reconstruction obtained in step 3 of Example 1;
[0019] Figure 3 is an aberration-corrected high-angle annular dark-field scanning transmission electron microscope of LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 of Example 1;
[0020] Figure 4 The aberration-corrected high-angle annular dark-field scanning transmission electron microscope of the LiYF4:25%Yb,0.5%Tm nanocrystal after the surface structure reconstruction treatment obtained in step 3 of Example 1;
[0021] Figure 5 It is the emission spectrum diagram of the LiYF4:25%Yb,0.5%Tm nanocrystal in Example 1 before and after the surface structure reconstruction under 980nm laser excitation.
[0022] Figure 6 is a transmission electron microscope photograph of LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 of Example 2;
[0023] Figure 7 is a transmission electron microscope photograph of LiYF4:25%Yb,0.5%Tm nanocrystals after surface structure reconstruction obtained in step 3 of Example 2;
[0024] Figure 8It is the emission spectrum diagram of the LiYF4:25%Yb,0.5%Tm nanocrystal in Example 2 before and after the surface structure reconstruction under 980nm laser excitation.
[0025] Fig. 9 is a transmission electron microscope photograph of NaYF4:25%Yb,0.5%Er nanocrystals obtained in step 1 of Example 3;
[0026] Fig.10 is a transmission electron microscope photograph of the NaYF4:25%Yb,0.5%Er nanocrystal after the surface structure reconstruction treatment obtained in step 3 of Example 3;
[0027] Fig.11 It is the emission spectrum diagram of the NaYF4:25%Yb,0.5%Er nanocrystal before and after the surface structure reconstruction under 980nm laser excitation in Example 3. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is described in detail below with reference to the accompanying drawings and examples, but the present invention is not limited to the scope of the examples.
[0029] Embodiment 1: The method for reconstructing the surface structure of rare earth-doped LiYF4 nanocrystals of this embodiment is carried out according to the following steps:
[0030] 1. Synthesis of LiYF4:25%Yb,0.5%Tm nanocrystals by thermal cracking method (the ratio of rare earth elements in the nanocrystals is Yb:Y:Tm=0.25:0.745:0.005, Yb and Tm are rare earth elements, replacing Y element doped in LiYF4 matrix material):
[0031] (1) 3 ml of deionized water, 3 ml of ethanol and 9 ml of cyclohexane were mixed uniformly to obtain solution A; 3 mmol of lithium oleate (LiOA) and a total of 1 mmol of YCl3·6H2O, YbCl3·6H2O and TmCl3·6H2O were weighed; wherein Yb:Y:Tm=0.25:0.745:0.005, and added to solution A, and then the temperature was raised to 70°C and kept at this temperature for 12 hours. After cooling, the liquid was separated into layers, and the upper organic phase was obtained and put back into a three-necked flask for later use, which was recorded as solution B;
[0032] (2) Add 4 mmol LiOA powder, 6 ml oleic acid and 15 ml 1-octadecene to solution B, stir and heat to 160°C under inert gas protection and maintain for 30 min to remove water;
[0033] (3) After cooling to room temperature, add 4 mmol NH4F powder, stir and heat to 80°C for 30 min to dissolve the powder;
[0034] (4) heating to 290°C, maintaining for 90 min, and then naturally cooling to room temperature to obtain solution C;
[0035] (5) Pour solution C into a centrifuge tube, add ethanol, and centrifuge at 8000 r / min for 5 min. Repeat the centrifugation three times and disperse it in cyclohexane to obtain 10 ml of cyclohexane dispersion of LiYF4:25% Yb,0.5% Tm nanocrystals.
[0036] 2. Preparation of rare earth ion Y 3+ Oleic acid / 1-octadecene precursor solution: Weigh 1.5 mmol of Y(CH3COO)3 and add it to a three-necked flask, mix it with 6 ml of oleic acid and 15 ml of 1-octadecene in the three-necked flask, and under argon protection, stir and heat to 160°C and maintain for 30 minutes to fully dissolve the raw materials to obtain a precursor solution;
[0037] 3. Mix 2 ml of LiYF4:25% Yb, 0.5% Tm nanocrystals dispersed in cyclohexane with 5 ml of precursor solution. Then, keep the mixture at 160°C for 30 min to remove cyclohexane and water, then raise the temperature to 290°C and keep for 1 h. After cooling to room temperature, pour the resulting liquid into a centrifuge tube, add ethanol, and centrifuge at 8000 r / min for 5 min. After repeated centrifugation 3 times, disperse it in cyclohexane to complete the surface structure reconstruction of rare earth-doped LiYF4 nanocrystals.
[0038] The transmission electron microscope photo of LiYF4:25%Yb,0.5%Tm nanocrystals prepared in step 1 of this embodiment 1 is as follows Figure 1 As shown in the transmission electron microscope photo of LiYF4:25%Yb,0.5%Tm nanocrystal after surface structure reconstruction treatment obtained in step 3, Figure 2 As shown, from Figure 1 and Figure 2 It can be seen that the LiYF4:25%Yb,0.5%Tm nanocrystals synthesized in Example 1 are uniform tetragonal nanoparticles, which are evenly dispersed and have a size of about 35 nm. Moreover, the particle size does not change significantly after the surface structure reconstruction treatment.
[0039] The aberration-corrected high-angle annular dark-field scanning transmission electron microscope of the LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 of this embodiment is as follows Figure 3 As shown in the figure, the aberration-corrected high-angle annular dark-field scanning transmission electron microscope of LiYF4:25%Yb,0.5%Tm nanocrystals after the surface structure reconstruction treatment obtained in step 3 is as follows: Figure 4 As shown. Figure 3 and Figure 4It can be seen that from the atomic level, before and after the surface structure reconstruction treatment, the surface amorphous part of the nanocrystals is reduced and the crystallinity is improved.
[0040] The emission spectra of the LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 and step 3 of this embodiment 1 before and after the surface structure reconstruction under 980nm laser excitation are as follows Figure 5 As shown, the nanoparticles emit fluorescence signals in multiple bands, and the emission wavelengths are mainly located at 480nm, 645nm and 793nm, indicating that the luminescence of rare earth ions is enhanced after the surface structure is reconstructed.
[0041] Embodiment 2: The method for reconstructing the surface structure of LiYF4 nanocrystals in this embodiment is carried out according to the following steps:
[0042] 1. Synthesis of LiYF4:25%Yb by coprecipitation method 3+ / 0.5%Tm 3+ Nanocrystals:
[0043] (1) 0.0.745 mmol of YCl3·6H2O, 0.25 mmol of YbCl3·6H2O and 0.005 mmol of TmCl3·6H2O were added to a 250 mL three-necked flask containing 6 mL of oleic acid (OA) and 15 mL of 1-octadecene (DOE). The mixture was heated to 160 °C under argon for 30 min to form a transparent solution and the residual water was removed;
[0044] (2) The solution was cooled to room temperature, 10 mL of a methanol solution containing 2.5 mmol LiOH and 4 mmol NH4F was slowly dripped into the flask and stirred for 30 min, and the solution was heated to 80 °C and maintained for 30 min to evaporate the methanol;
[0045] (3) The solution was heated to 300°C and kept under argon for 1.5 hours. After cooling to room temperature, it was dissolved in cyclohexane and then precipitated with alcohol. This process was repeated three times and dissolved in 10 mL of cyclohexane to obtain LiYF4:25% Yb 3+ / 0.5%Tm 3+ Cyclohexane dispersion of nanocrystals, set aside;
[0046] 2. Preparation of rare earth ions Lu 3+ Oleic acid / 1-octadecene precursor solution: weigh 1.5 mmol of LuCl3 and add it to a three-necked flask, mix it with 6 ml of oleic acid and 15 ml of 1-octadecene in the three-necked flask, and under argon protection, stir and heat to 160°C and maintain for 30 minutes to fully dissolve the raw materials to obtain a precursor solution;
[0047] 3. Mix 2 ml of LiYF4:25% Yb, 0.5% Tm nanocrystals dispersed in cyclohexane with 5 ml of precursor solution, then keep it at 160°C for 30 min to remove cyclohexane and water in the mixture, then heat it to 290°C and keep it for 1 h. After cooling to room temperature, pour the resulting liquid into a centrifuge tube, add ethanol, centrifuge at 8000 r / min for 5 min, repeat the centrifugation 3 times, and disperse it in cyclohexane to complete LiYF4:25% Yb 3+ / 0.5%Tm 3+ Nanocrystal surface structure reconstruction.
[0048] The transmission electron microscope photo of LiYF4:25%Yb,0.5%Tm nanocrystals prepared in step 1 of this embodiment 2 is as follows Figure 6 As shown in the transmission electron microscope photo of LiYF4:25%Yb,0.5%Tm nanocrystal after surface structure reconstruction treatment obtained in step 3, Figure 7 As shown, from Figure 6 and Figure 7 It can be seen that the LiYF4:25%Yb,0.5%Tm nanocrystals synthesized in Example 2 are uniform tetragonal nanoparticles, which are evenly dispersed and have a size of about 25 nm. Moreover, the particle size does not change significantly after the surface structure reconstruction treatment.
[0049] The emission spectra of the LiYF4:25%Yb,0.5%Tm nanocrystals obtained in step 1 and step 3 of Example 2 before and after surface structure reconstruction under 980nm laser excitation are as follows Figure 8 As shown, the nanoparticles emit fluorescence signals in multiple bands, and the emission wavelengths are mainly located at 480nm, 645nm and 793nm, indicating that the luminescence of rare earth ions is enhanced after the surface structure is reconstructed.
[0050] Embodiment 3: The method for reconstructing the surface structure of NaYF4 nanocrystals of this embodiment is carried out according to the following steps:
[0051] 1. Synthesis of NaYF4:25% Yb by coprecipitation method 3+ / 0.5%Er 3+ Nanocrystals:
[0052] (1) 0.52 mmol of YCl3·6H2O, 0.40 mmol of YbCl3·6H2O and 0.08 mmol of ErCl3·6H2O were added into a 250 mL three-necked flask containing 6 mL of oleic acid (OA) and 15 mL of 1-octadecene (DOE), and the mixture was heated to 160 °C under argon. A transparent solution was formed in 30 minutes and the residual water was removed;
[0053] (2) The solution was cooled to room temperature, 10 mL of a methanol solution containing NaOH (2.5 mmol) and NH4F (4 mmol) was slowly dripped into the flask and stirred for 30 minutes;
[0054] (3) The solution was heated to 80°C and maintained for 30 minutes to evaporate the methanol. The solution was heated to 300°C and maintained under argon for 1.5 hours. After cooling to room temperature, it was first dissolved in cyclohexane and then precipitated with alcohol. This was repeated three times and dissolved in 10 mL of cyclohexane to obtain NaYF4:25% Yb 3+ / 0.5%Er 3+ Cyclohexane dispersion of nanocrystals, set aside;
[0055] 2. Preparation of rare earth ion Y 3+ Oleic acid / 1-octadecene precursor solution: weigh 1.5 mmol of Gd(CH3COO)3 and add it to a three-necked flask, mix it with 6 ml of oleic acid and 15 ml of 1-octadecene in the three-necked flask, and under argon protection, stir and heat to 160°C and maintain for 30 minutes to fully dissolve the raw materials to obtain a precursor solution;
[0056] 3. Disperse 2 ml of NaYF4:25% Yb in cyclohexane 3+ / 0.5%Er 3+ The nanocrystals were mixed with 5 ml of precursor solution; then, the mixture was kept at 160°C for 30 minutes to remove cyclohexane and water, then heated to 290°C and kept for 1 hour. After cooling to room temperature, the resulting liquid was poured into a centrifuge tube, ethanol was added, and centrifuged at 8000 r / min for 5 minutes. After repeated centrifugation for 3 times, the mixture was dispersed in cyclohexane to complete the reconstruction of the nanocrystal surface structure.
[0057] The transmission electron microscope photo of the NaYF4:25%Yb,0.5%Er nanocrystal prepared in step 1 of this embodiment 3 is as follows Fig. 9 As shown in the transmission electron microscope photo of NaYF4:25%Yb,0.5%Er nanocrystal after surface structure reconstruction treatment obtained in step 3, Fig.10 As shown, from Fig. 9 and Fig.10 It can be seen that the NaYF4:25%Yb,0.5%Er nanocrystals synthesized in Example 2 are uniform hexagonal nanoparticles, which are evenly dispersed and have a size of about 25 nm. Moreover, the particle size does not change significantly after the surface structure reconstruction treatment.
[0058] The emission spectra of the NaYF4:25%Yb,0.5%Er nanocrystals obtained in step 1 and step 3 of this embodiment 3 before and after surface structure reconstruction under 980nm laser excitation are as follows Fig.11As shown, the nanoparticles emit fluorescence signals in multiple bands, and the emission wavelengths are mainly located at 525nm, 550nm and 660nm, indicating that the luminescence of rare earth ions is enhanced after the surface structure is reconstructed.
Claims
1. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals, characterized in that The method proceeds as follows:
1. A precursor solution is prepared by using a mixed solution of oleic acid and 1-octadecene as a solvent and a soluble salt of an inert rare earth ion as a solute; wherein the inert rare earth ion is yttrium, lutetium, gadolinium or lanthanum; 2. Mixing the initial rare earth doped fluoride nanocrystal cyclohexane dispersion with the precursor solution, wherein the ratio of the amount of trivalent cations in the initial rare earth doped fluoride nanocrystal cyclohexane dispersion to the amount of rare earth ions in the precursor solution is 1:(1-8); then, keeping the mixture at a temperature of 100-180°C for 10-30 minutes to remove cyclohexane and water in the mixture, then heating it to 200-300°C and keeping it for 5-90 minutes, then cooling it to room temperature, pouring the resulting liquid into a centrifuge tube, adding ethanol, and centrifuging and washing it at a speed of 5000-10000 r / min for 5-15 minutes; after repeating the centrifugal washing 2-3 times, dispersing it in cyclohexane to complete the surface structure reconstruction of the rare earth doped fluoride nanocrystals.
2. The method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1, characterized in that: The size of the rare earth doped fluoride nanocrystals in the initial rare earth doped fluoride nanocrystal cyclohexane dispersion is 5 to 60 nm.
3. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1 or 2, characterized in that: The volume ratio of oleic acid to 1-octadecene in the mixed solution of oleic acid and 1-octadecene in step 1 is 1:(1-3).
4. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1 or 2, characterized in that: The precursor solution described in step 1 contains 0.5 to 4 mmol of inert rare earth ions per 10 ml of the precursor solution.
5. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1 or 2, characterized in that: The soluble salt of the inert rare earth ion in step 1 is the acetate or chloride of the inert rare earth ion.
6. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1 or 2, characterized in that: The preparation method of the precursor solution described in step 1 is as follows: add a soluble salt of an inert rare earth ion to a mixed solution of oleic acid and 1-octadecene, and under the protection of an inert gas such as nitrogen or argon, stir and heat to 100-160° C. and maintain for 10-60 minutes to dissolve the raw materials to obtain a precursor solution.
7. A method for reconstructing the surface structure of rare earth-doped fluoride nanocrystals according to claim 1 or 2, characterized in that: The initial rare earth-doped fluoride nanocrystals described in step 2 are, for example, LiYF4, LiLuF4, LiGdF4, NaYF4 or NaGdF4.
Citation Information
Patent Citations
Super-enhanced luminescent upper conversion core shell nanocrystalline material and preparation method thereof
CN107603625A
Method for improving luminous intensity of rare earth alkali metal fluoride nanocrystals