Zero-emission full-recovery treatment method for waste plastics

By adjusting the parameters of the wave source generator and reactor in the wave cracking reactor, the cracking degree and efficiency of waste plastics are improved, the problems of low cracking degree and efficiency in the existing technology are solved, and efficient recycling and resources of waste plastics are realized. High-value processing.

CN119081726APending Publication Date: 2024-12-06CHINA RE OIL TECHNOLOGY (BEIJING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411403839.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-10-10
Filing Date
2024-10-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has low cracking degree and cracking efficiency during wave cracking, making it difficult to effectively treat waste plastics, resulting in low resource utilization efficiency.

Method used

By pretreating waste plastics, including water removal, density and crushing, and adjusting the electromagnetic parameters and reactor parameters of the wave source generator in the wave cracking reactor, controlling the phase angle difference value and energy density, improving the wave cracking efficiency and cracking to achieve oil and gas separation and solid recovery.

Benefits of technology

It has achieved 100% recycling of waste plastics without secondary pollution, small investment in equipment, simple process, low cost, and significant energy, environmental and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081726A_ABST
    Figure CN119081726A_ABST
Patent Text Reader

Abstract

The invention relates to a zero-emission full-recovery treatment method for waste plastics. The method comprises the following steps: pretreating a waste plastic raw material; feeding the pretreated raw materials into a wave cracking reaction kettle, adjusting electromagnetic parameters of N wave source generators in the wave cracking reaction kettle, and controlling the N wave source generators to be circularly started, the electromagnetic parameters at least comprise the single-time starting duration t < single > of the wave source generators and the phase angle difference value delta theta between the two wave source generators with adjacent irradiation time periods; adjusting parameters of the reaction kettle, and starting the wave cracking reaction kettle; recovering a product of the wave cracking reaction kettle; wherein the value range of the phase angle difference value delta theta is 21 degrees to 23 degrees; after the wave cracking reaction kettle is started, the energy density in the wave cracking reaction kettle is 130-220Wh / L. According to the invention, by reasonably controlling the electromagnetic parameters of the wave source generator and the reaction kettle parameters in the wave cracking reaction kettle, the wave cracking efficiency and the cracking degree can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention claims the priority of the Chinese patent application filed with the Chinese Patent Office on October 10, 2023, with application number 202311307350.8 and application name “Zero-emission full recycling method for waste plastics”, the entire contents of which are incorporated by reference into the present invention. Technical Field

[0002] The invention belongs to the technical field of resource utilization and high-value treatment of waste plastics, and specifically relates to a zero-emission and full-recycling treatment method for waste plastics. Background Art

[0003] Energy conservation, environmental protection, low-carbon emission reduction and renewable energy development have always been the key support targets of my country's development planning outline. There are three relatively concentrated sources of waste plastics: one is the country's relatively large plastic distribution centers; the second is waste plastics in domestic waste landfills; and the third is industrial waste and scrapped electronic appliances, home appliances and automobile plastic products.

[0004] 1. There are about 34 plastic distribution centers in China, mainly distributed in the coastal and more developed eastern regions. They are raw material trading markets for the recycled plastics industry, and most of them have been in operation for three to four decades.

[0005] 2. Waste plastics in domestic waste landfills. The content of waste plastics in domestic waste landfills is 10%-25%, and the content of waste plastics in tourist cities is even higher. In order to prevent groundwater pollution, the government has ordered landfills to implement regular anti-seepage sanitary landfills. Those informal landfills must dig out the garbage again and implement regular landfills in accordance with national policies. Take Beijing as an example. Beijing has implemented harmless sanitary landfill of domestic waste since 2006. At present, Beijing has 18 waste treatment plants, which process more than 20,000 tons of domestic waste per day. According to statistics, the domestic waste landfills that have been closed in my country cover an area of ​​more than 3 million mu, with a total landfill of more than 4 billion tons of domestic waste. Calculated based on a 20% plastic content, the total amount of waste plastics buried in the landfills is more than 800 million tons.

[0006] 3. Industrial waste and scrapped electronic appliances, household appliances and automobile plastic products. The world produces more than 50 million tons of electronic waste each year, and China produces 2.3 million tons each year. In addition, the annual consumption of automobile plastics has reached 400,000 tons, and the annual consumption of plastics for electronic appliances and household appliances has reached more than 1 million tons. These products have become one of the important sources of waste plastics after being scrapped.

[0007] It can be seen that my country has sufficient sources of waste plastics. If we can achieve high-value recycling of resources, it will not only solve the "white pollution" problem, but also increase the area of ​​arable land and turn all the land occupied by domestic waste landfills into fertile fields. At the same time, it can greatly alleviate my country's energy supply security and achieve high-value energy utilization of waste plastics.

[0008] Wave cracking technology uses fixed-frequency physical waves as its power source, and breaks organic macromolecules into organic small molecules by resonating and breaking CC chemical bonds. It can decompose waste plastics into natural gas, fuel oil and solid carbon.

[0009] However, the degree and efficiency of the wave cracking process are still technical issues that need to be solved urgently. Summary of the invention

[0010] The purpose of the present invention is to provide an industrial application method for zero-emission and full recycling of waste plastics, which has a simple process flow, small equipment investment, high product added value, significant economic benefits, and very superior energy benefits, environmental benefits and social benefits. At the same time, the wave cracking efficiency and cracking degree can be greatly improved by reasonably controlling the electromagnetic parameters of the wave source generator and the reactor parameters in the wave cracking reactor.

[0011] The technical solution of the present invention is: an industrial application method for zero-emission full recycling of waste plastics, comprising the following steps:

[0012] Step S1, pre-treating the waste plastic raw material, wherein the pre-treatment process at least includes dehydration, densification and crushing;

[0013] Step S2, feeding the pretreated raw material into the wave cracking reactor, adjusting the electromagnetic parameters of the N wave source generators in the wave cracking reactor, and controlling the N wave source generators to cyclically start, wherein the electromagnetic parameters at least include the single start time t of the wave source generator 单 , a phase angle difference Δθ between two wave source generators with adjacent irradiation time periods;

[0014] Step S3, adjusting the reactor parameters, starting the wave cracking reactor, recovering the top product of the wave cracking reactor, completing oil and gas separation by four-stage condensation, and recovering the gas product and liquid product of wave cracking;

[0015] Step S4, using a magnetic separator to respectively recover the activated carbon, metal and magnetic oxide at the bottom of the wave cracking reactor;

[0016] The phase angle difference Δθ ranges from 21° to 23°.

[0017] After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.

[0018] According to a technical solution of the present invention, the step S1 specifically includes:

[0019] The waste plastics are pre-treated to remove water and densify, and the bulk density or apparent density of the waste plastics is increased to 0.5g / cm 3 The shape of the pre-treated raw materials is spherical, cylindrical, square or irregular shaped fluid plastic particles.

[0020] According to a technical solution of the present invention, in step S2, the wave cracking reactor adopts a vertical structure, and the pretreated raw materials are transported from a low position to a high position by a conveyor, and then transported from the high position into the wave cracking reactor.

[0021] According to a technical solution of the present invention, in step S2, the electromagnetic wave emitted by any of the wave source generators is expressed as:

[0022] E(t i )=A i ·sin(2πft+θ i )

[0023] Among them, t i represents the i-th time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, and f represents frequency, then:

[0024] Δθ=θ i+1 -θ i .

[0025] According to a technical solution of the present invention, the single opening time length t of any of the wave source generators 单 It is 30s to 200s.

[0026] According to a technical solution of the present invention, the step S3 specifically includes:

[0027] After the wave cracking reactor is started, a large amount of oil and gas vapor will be discharged from the top of the wave cracking reactor, and the oil and gas separation will be completed through four-stage condensation. The heavy combustion oil component is first cooled by an air condenser; then cooled by a first-stage water condenser to obtain a diesel component; then cooled by a second-stage water condenser to obtain a gasoline component; and finally cooled by a third-stage water condenser to obtain a naphtha component.

[0028] The non-condensable oil and gas parts are first passed through a purification tower to remove impurities, and then compressed and liquefied by a compressor to obtain a liquefied gas product. The non-compressible combustible gas is stored in a pressure vessel tank to obtain a natural gas product.

[0029] According to a technical solution of the present invention, a wave absorbing material is arranged in the wave cracking reactor, and the amount of the wave absorbing material accounts for 0.1%-10% of the total raw material weight in terms of mass percentage;

[0030] The wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor along with the raw materials after pretreatment.

[0031] According to a technical solution of the present invention, the reaction kettle parameters at least include the pressure inside the kettle, the temperature inside the kettle and the wave cracking time.

[0032] According to a technical solution of the present invention, the pressure in the kettle is 2800Pa-5000Pa, the temperature in the kettle is 300°C-400°C, and the wave cracking time is 40min-200min.

[0033] According to a technical solution of the present invention, the step S4 specifically includes:

[0034] The solid components at the bottom of the wave cracking reactor are collected, and the solid components are magnetically separated from metals and magnetic oxides by a magnetic separator to obtain carbon-containing solids after magnetic separation. The carbon content of the carbon-containing solids is higher than 70%.

[0035] The beneficial effects of the present invention are:

[0036] The present invention can realize 100% recycling of waste plastics without generating secondary pollution. Solid waste plastics can be completely decomposed into organic oil and gas small molecule products, and the metals carried in plastic products, such as springs, screws, nuts, iron wires and other inorganic metal materials, can be completely unaffected and recovered and regenerated from the bottom of the wave cracking reactor, thereby realizing zero-emission, full recycling and high-value utilization of waste plastics. The entire industrial process has no carbon consumption, no three wastes, and 100% full recycling. The method has small equipment investment, simple process, low cost, high added value, no secondary pollution, significant economic benefits, easy large-scale industrial processing, and has very good energy benefits, environmental benefits and social benefits.

[0037] By rationally controlling the electromagnetic parameters of the wave source generator and the reactor parameters in the wave cracking reactor, the wave cracking efficiency and cracking degree can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A flowchart schematically showing a method for zero-emission and full recycling of waste plastics according to one embodiment of the present invention;

[0039] Figure 2 A schematic diagram showing the change of the degree of cleavage over time in Example 1;

[0040] Figure 3 A schematic diagram showing the change of the gas product ratio over time in Example 1;

[0041] Figure 4 A schematic diagram showing the change of the degree of cleavage over time in Example 2;

[0042] Figure 5 A schematic diagram showing the change of the degree of cleavage over time in Example 3;

[0043] Figure 6 A schematic diagram showing the change of the degree of cleavage over time in Example 4;

[0044] Figure 7 A graph schematically showing the relationship between the degree of fragmentation and the relative value of the phase angle. DETAILED DESCRIPTION

[0045] The description of the embodiments of this specification should be combined with the corresponding drawings, which should be considered as part of the complete specification. In the drawings, the shape or thickness of the embodiments may be enlarged and indicated for simplification or convenience. Furthermore, the parts of each structure in the drawings will be described separately. It is worth noting that the elements not shown in the drawings or not described in words are in a form known to ordinary technicians in the relevant technical field.

[0046] The description of the embodiments herein and any reference to directions and orientations are only for the convenience of description and are not to be construed as any limitation on the scope of protection of the present invention. The following description of the preferred embodiments may involve combinations of features, which may exist independently or in combination, and the present invention is not particularly limited to the preferred embodiments. The scope of the present invention is defined by the claims.

[0047] In order to make the technical means, creative features, objectives and beneficial effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0048] like Figures 1 to 7 As shown, according to one embodiment of the present invention, a method for zero-emission and full recycling of waste plastics of the present invention comprises the following steps:

[0049] Step S1, pre-treating the waste plastic raw materials, the pre-treatment process at least includes dehydration, densification and crushing, specifically including:

[0050] The waste plastics are pre-treated to remove water and densify, and the bulk density or apparent density of the waste plastics is increased to 0.5g / cm 3 The shape of the pre-treated raw materials is spherical, cylindrical, square or irregular shaped fluid plastic particles.

[0051] Step S2, feeding the pretreated raw material into the wave cracking reactor, adjusting the electromagnetic parameters of the N wave source generators in the wave cracking reactor, and controlling the N wave source generators to cyclically start, wherein the electromagnetic parameters at least include the single start time t of the wave source generator 单 , a phase angle difference Δθ between two wave source generators with adjacent irradiation time periods;

[0052] The pre-treated raw materials are transported from a low position to a high position by a conveyor, and then transported from the high position to a wave cracking reactor. The wave cracking reactor adopts a vertical structure, and N wave source generators are arranged in the reactor. The wave source generators are cyclically turned on or off in different time periods. For example, when the second wave source generator is turned on, the first wave source generator, the third wave source generator...the Nth wave source generator are all turned off. The single opening time length t of any of the wave source generators 单 It is 30s to 200s.

[0053] The electromagnetic wave emitted by any of the wave source generators is expressed as:

[0054] E(t i )=A i ·sin(2πft+θ i )

[0055] Among them, t i represents the i-th time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, and f represents frequency, then:

[0056] Δθ=θ i+1 -θ i .

[0057] It is understandable that when the single opening time t 单 When it is set to 100s and the phase angle difference Δθ is set to 21°, in the first time period (the first 100s), the electromagnetic wave emitted by the first wave source generator is expressed as: E(t1) = A1·sin(2πft+θ1). From the 101st second, the first wave source generator is turned off and the second wave source generator is turned on. The electromagnetic wave emitted by the second wave source generator is expressed as: E(t2) = A2·sin(2πft+θ2). Under normal circumstances, A1 = A2, and Δθ = θ2-θ1 = 21°; and from the 201st second, the second wave source generator is turned off and the third wave source generator is turned on, then Δθ = θ3-θ2 = 21°, and so on. When the Nth wave source generator is turned off and the set wave splitting time has not been reached, the first wave source generator is turned on again for the next cycle.

[0058] Typically, the value range of N is 3 to 20, preferably, the value range is 4 to 10.

[0059] In addition, the first wave source generator, the second wave source generator, the third wave source generator...the Nth wave source generator can be regarded as the first type of wave source generator, the second type of wave source generator, the third type of wave source generator...the Nth type of wave source generator. Multiple wave source generators of each type can be set and turned on or off at the same time to improve the wave splitting efficiency.

[0060] A wave absorbing material is arranged in the wave cracking reaction kettle, and the amount of the wave absorbing material accounts for 0.1%-10% of the total raw material weight in terms of mass percentage; the wave absorbing material is nano iron oxide.

[0061] The wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor along with the raw materials after pretreatment.

[0062] The phase angle difference Δθ ranges from 21° to 23°.

[0063] Step S3, adjusting the reactor parameters, starting the wave cracking reactor, recovering the top product of the wave cracking reactor, completing oil and gas separation by four-stage condensation, and recovering the gas product and liquid product of wave cracking, specifically includes:

[0064] After the wave cracking reactor is started, a large amount of oil and gas vapor will be discharged from the top of the wave cracking reactor, and the oil and gas separation will be completed through four-stage condensation. The heavy combustion oil component is first cooled by an air condenser; then cooled by a first-stage water condenser to obtain a diesel component; then cooled by a second-stage water condenser to obtain a gasoline component; and finally cooled by a third-stage water condenser to obtain a naphtha component.

[0065] The non-condensable oil and gas parts are first passed through a purification tower to remove impurities, and then compressed and liquefied by a compressor to obtain a liquefied gas product. The non-compressible combustible gas is stored in a pressure vessel tank to obtain a natural gas product.

[0066] After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.

[0067] The reactor parameters include at least the reactor pressure, reactor temperature and wave cracking time.

[0068] Typically, the pressure in the kettle is 2800Pa-5000Pa, the temperature in the kettle is 300°C-400°C, and the wave cracking time is 40min-200min; and the wave cracking time refers to the time when no cracking reaction occurs in the wave cracking reactor.

[0069] Step S4, using a magnetic separator to respectively recover the activated carbon, metal and magnetic oxide at the bottom of the wave cracking reactor, specifically comprising:

[0070] The solid components at the bottom of the wave cracking reactor are collected, and the solid components are magnetically separated from metals and magnetic oxides by a magnetic separator to obtain carbon-containing solids after magnetic separation. The carbon content of the carbon-containing solids is higher than 70%.

[0071] Four groups of specific implementation methods are given below based on the above-mentioned waste plastic zero-emission full recycling method to specifically illustrate the waste plastic zero-emission full recycling method of the present invention. In the following four embodiments, waste plastics such as disposable tableware, foam packaging materials, and electrical appliance housings are used as the main raw materials, and the main component is polystyrene (PS). In order to save time and facilitate detection, the metal products in the raw materials are first shaved off, and the above waste plastic raw materials are pretreated as in the above-mentioned step S1.

[0072] It should also be noted that the cracking degree in the present invention is expressed as: cracking degree = (mass of gas product + mass of liquid product + mass of solid carbon) / mass of raw material × 100%; and for the recovery rate involved in the present invention, the recovery rate = (mass of gas product + mass of liquid product + mass of solid carbon) / (mass of initial raw material - mass of remaining solid) × 100%.

[0073] Example 1

[0074] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the N wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 150s, Δθ=22°, and the number of wave source generators N=5.

[0075] The wavelength is set to 2300m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 110kHz, the wave cracking temperature is 350℃, the wave cracking pressure is 3000Pa, the energy density is 200Wh / L, the wave cracking time is 200min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.

[0076] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 94 kg of four fuel oils (including 31 kg of heavy oil components, 37 kg of diesel components, 25.4 kg of gasoline components, and 0.6 kg of naphtha components), 1 kg of liquefied gas, about 1 kg of natural gas, 4 kg of solid carbon and uncracked solids, the product recovery rate was close to 100%, and the cracking degree was more than 99%. During the wave cracking process, the products were continuously analyzed, and the following were obtained: Figure 2 and Figure 3The recovery curve and gas product ratio curve are shown, where the gas ratio refers to the percentage of the obtained gas to all the initial raw materials. After the wave cracking time reaches 45 minutes, almost no gas product is produced.

[0077] Example 2

[0078] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the N wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 150s, Δθ=15°, and the number of wave source generators N=7.

[0079] The wavelength is set to 2300m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 120kHz, the wave cracking temperature is 360℃, the wave cracking pressure is 3200Pa, the energy density is 200Wh / L, the wave cracking time is 200min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.

[0080] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: a total of 25.1 kg of four fuel oils (including 8.2 kg of heavy oil components, 9.5 kg of diesel components, 7.3 kg of gasoline components, and 0.1 kg of naphtha components), 0.1 kg of liquefied gas, about 0.1 kg of natural gas, 1.5 kg of solid carbon, and 73.2 kg of uncracked solids. The product recovery rate was close to 100%, and the cracking degree was 26.8%. During the wave cracking process, the products were continuously analyzed, and the following data were obtained: Figure 4 In the recovery rate curve shown, the gas product accounts for a small proportion and no curve is drawn. After the wave cracking time reaches 150 minutes, almost no gas product is produced.

[0081] Example 3

[0082] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the N wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 150s, Δθ=24°, and the number of wave source generators N=6.

[0083] The wavelength is set to 2300m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 130kHz, the wave cracking temperature is 360℃, the wave cracking pressure is 3000Pa, the energy density is 200Wh / L, the wave cracking time is 200min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.

[0084] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: the total amount of four fuel oils was 64.9 kg (including 21.4 kg of heavy oil components, 22.2 kg of diesel components, 21 kg of gasoline components, and 0.3 kg of naphtha components), 0.3 kg of liquefied gas, about 0.4 kg of natural gas, 2.3 kg of solid carbon, and 32.1 kg of uncracked solids. The product recovery rate was close to 100%, and the cracking degree was 67.9%. During the wave cracking process, the products were continuously analyzed, and the following were obtained: Figure 5 In the recovery rate curve shown, the gas product accounts for a small proportion and no curve is drawn. After the wave cracking time reaches 80 minutes, almost no gas product is produced.

[0085] Example 4

[0086] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the N wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 150s, Δθ=28°, and the number of wave source generators N=5.

[0087] The wavelength is set to 2300m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 100kHz, the wave cracking temperature is 350℃, the wave cracking pressure is 3000Pa, the energy density is 200Wh / L, the wave cracking time is 200min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.

[0088] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 24.2 kg of four fuel oils in total (8.1 kg of heavy oil components, 8.9 kg of diesel components, 7.1 kg of gasoline components, and 0.1 kg of naphtha components), 0.1 kg of liquefied gas, about 0.1 kg of natural gas, 1.3 kg of solid carbon, 74.3 kg of uncracked solids, the product recovery rate was close to 100%, and the cracking degree was 25.7%. During the wave cracking process, the products were continuously analyzed, and the following were obtained: Figure 6 In the recovery rate curve shown, the gas product accounts for a small proportion and no curve is drawn. After the wave cracking time reaches 90 minutes, almost no gas product is produced.

[0089] It can be seen that the method provided by the present invention can achieve nearly 100% conversion of waste plastics into energy products, which has far-reaching applications in ensuring national energy supply security. At the same time, the economic benefits brought by the invention are very significant. Based on the above four embodiments and the actual production process, the following diagram is drawn: Figure 7The relationship between the cracking degree and the relative value of the phase angle is shown. By reasonably controlling the electromagnetic parameters of the wave source generator and the reactor parameters in the wave cracking reactor, the wave cracking efficiency and cracking degree can be greatly improved.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for zero-emission and full recycling of waste plastics. It is characterized in that The following steps are involved: Step S1, pre-treating the waste plastic raw material, wherein the pre-treatment process at least includes dehydration, densification and crushing; Step S2, feeding the pretreated raw material into the wave cracking reactor, adjusting the electromagnetic parameters of the N wave source generators in the wave cracking reactor, and controlling the N wave source generators to cyclically start, wherein the electromagnetic parameters at least include the single start time t of the wave source generator 单 , a phase angle difference Δθ between two wave source generators with adjacent irradiation time periods; Step S3, adjusting the reactor parameters, starting the wave cracking reactor, recovering the top product of the wave cracking reactor, completing oil and gas separation by four-stage condensation, and recovering the gas product and liquid product of wave cracking; Step S4, using a magnetic separator to respectively recover the activated carbon, metal and magnetic oxide at the bottom of the wave cracking reactor; Wherein, the phase angle difference Δθ has a value range of 21° to 23°; After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.

2. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that The step S1 specifically includes: The waste plastics are pre-treated to remove water and densify, and the bulk density or apparent density of the waste plastics is increased to 0.5g / cm 3 The shape of the pre-treated raw materials is spherical, cylindrical, square or irregular shaped fluid plastic particles.

3. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that In the step S2, the wave cracking reactor adopts a vertical structure, and the pretreated raw materials are transported from a low position to a high position by a conveyor, and then transported from the high position into the wave cracking reactor.

4. A method for zero-emission and full recycling of waste plastics according to claim 1 or 3, It is characterized in that In step S2, the electromagnetic wave emitted by any of the wave source generators is expressed as: E(t i )=A i ·sin(2πft+θ i ) Among them, t i represents the i-th time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, and f represents frequency, then: Δθ=θ i+1 -θ i 。 5. A method for zero-emission and full recycling of waste plastics according to claim 4, It is characterized in that The single opening time t of any of the wave source generators 单 It is 30s to 200s.

6. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that The step S3 specifically includes: After the wave cracking reactor is started, a large amount of oil and gas vapor will be discharged from the top of the wave cracking reactor, and the oil and gas separation will be completed through four-stage condensation. The heavy combustion oil component is first cooled by an air condenser; then cooled by a first-stage water condenser to obtain a diesel component; then cooled by a second-stage water condenser to obtain a gasoline component; and finally cooled by a third-stage water condenser to obtain a naphtha component. The non-condensable oil and gas parts are first passed through a purification tower to remove impurities, and then compressed and liquefied by a compressor to obtain a liquefied gas product. The non-compressible combustible gas is stored in a pressure vessel tank to obtain a natural gas product.

7. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that The wave absorbing material is arranged in the wave cracking reaction kettle, and the amount of the wave absorbing material accounts for 0.1%-10% of the total raw material weight in terms of mass percentage; The wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor along with the raw materials after pretreatment.

8. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that The reactor parameters at least include the reactor internal pressure, the reactor internal temperature and the wave cracking time.

9. A method for zero-emission and full recycling of waste plastics according to claim 8, It is characterized in that The pressure in the kettle is 2800Pa-5000Pa, the temperature in the kettle is 300°C-400°C, and the wave cracking time is 40min-200min.

10. A method for zero-emission and full recycling of waste plastics according to claim 1, It is characterized in that The step S4 specifically includes: The solid components at the bottom of the wave cracking reactor are collected, and the solid components are magnetically separated from metals and magnetic oxides by a magnetic separator to obtain carbon-containing solids after magnetic separation. The carbon content of the carbon-containing solids is higher than 70%.