Method for leaching copper and cobalt from high-iron-copper-cobalt material

By pretreatment, acid leaching and filtration of high-speed iron copper-cobalt material, using ammonium hydrogen fluoride and sodium chlorate as additives and oxidizing agents, the problems of complex process and toxic gases in the prior art are solved, and high-efficiency copper-cobalt is achieved Leaching and high recovery rates.

CN119082453APending Publication Date: 2024-12-06ZHONG QING JI & YE LIAN YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193576.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing methods of extracting metals from high-speed rail copper and cobalt materials have problems such as complex process flow, generation of toxic gases, high processing costs and limited production capacity.

Method used

The methods of pretreatment, acid leaching and filtration are adopted, including crushing and grinding of high-speed iron copper and cobalt material, adding water to mix slurry, adding concentrated sulfuric acid and ammonium hydrogen fluoride for reaction, and adding sodium chlorate solution at high temperature. The pH value was controlled for filtration, using ammonium hydrogen fluoride and sodium chlorate as additives and oxidants.

Benefits of technology

It realizes efficient leaching of copper and cobalt, with a short process and a high leaching rate of copper and cobalt, and iron impurities are mainly left in the slag, with simple operation and high metal recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a method for leaching copper and cobalt from a high-iron-copper-cobalt material, belongs to the technical field of chemical extraction, aims to solve the problems of low efficiency and low leaching rate of extracting copper and cobalt from the high-iron-copper-cobalt material, and comprises the steps of grinding pretreatment, acid leaching treatment after dissolution, filtration treatment and the like, ammonium bifluoride is used as an additive, sodium chlorate is used as an oxidizing agent, the process is short, and the cost is low. And the copper-cobalt leaching rate is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical extraction, and more specifically, particularly relates to a method for leaching copper and cobalt from high-iron copper and cobalt materials. Background Art

[0002] With the rapid development of new energy, new materials and other industries, the demand for metals such as cobalt and copper is growing. However, the grade of cobalt mining is getting lower and lower, and the ore composition liquid is becoming more and more complex. At present, there are two methods for extracting metals from high-iron and copper cobalt materials: acid leaching and chlorine leaching. The former process is to add enough acid to control the pH value at about 1.0, and sometimes a reducing agent is added to make almost all the metal elements in the cobalt material leached, and then remove the impurities such as iron, aluminum, calcium, and magnesium in the leachate. A large amount of NO, NO2, SO2 and other toxic gases will be produced during the leaching process. The latter method takes a long time for the entire leaching process, but chlorine is produced during the production process, which limits the production capacity of the equipment, has a high processing cost and causes great air pollution.

[0003] Therefore, in view of this, the existing structure and defects are studied and improved, and a method for leaching copper and cobalt from high-iron copper and cobalt materials is provided, in order to achieve a more practical purpose. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for leaching copper and cobalt from a high-iron copper and cobalt material to solve the above problems.

[0005] The purpose and effect of the method for leaching copper and cobalt from high-iron copper and cobalt materials of the present invention are achieved by the following specific technical means:

[0006] A method for leaching copper and cobalt from a high-iron copper and cobalt material comprises the following steps:

[0007] 1) Pretreatment: crushing and grinding the high iron, copper and cobalt raw materials;

[0008] 2) Dissolving; taking the pretreated high iron copper cobalt material, adding water to slurry and stirring;

[0009] 3) Acid leaching treatment: add concentrated sulfuric acid to the stirred solution, heat it in water and react for 1-3 hours, then add ammonium bifluoride and react for 0.5-1.5 hours, and at the same time take sodium chlorate solution and add it dropwise to the reaction solution to continue the reaction;

[0010] 4) Filtration; the solution after the reaction was filtered when the pH value was 2.2-2.6 after 1 hour, and the filter residue was washed.

[0011] Furthermore, the volume ratio of the cobalt material to water in the water slurry of step 2 is 7:1.

[0012] Furthermore, in step 3, concentrated sulfuric acid is reacted for 2 hours, and ammonium bifluoride is added and reacted for 1 hour.

[0013] Further, in step 4, filtration is performed when the pH value is 2.4.

[0014] Furthermore, taking 98% concentration sulfuric acid solution as an example, the ratio of high iron, copper and cobalt raw materials to concentrated sulfuric acid is 1g: 0.36ml-0.43ml; the ratio of high iron, copper and cobalt raw materials to ammonium bifluoride is 25g: 1g-3g; the ratio of high iron, copper and cobalt raw materials to sodium chlorate is 50g: 26g-47.2g.

[0015] Furthermore, the usage ratio of high iron copper cobalt raw material to concentrated sulfuric acid, ammonium bifluoride and sodium chlorate is 50g:20ml:4g:40g.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] With ammonium bifluoride as additive and sodium chlorate as oxidant, the process is short and the copper and cobalt leaching rate is high. DETAILED DESCRIPTION

[0018] The following examples are used to illustrate the present invention, but they are not intended to limit the scope of the present invention.

[0020] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0021] Example:

[0022] The present invention provides a method for leaching copper and cobalt from a high-iron copper and cobalt material, comprising the following steps:

[0023] Pretreatment: The high-iron copper and cobalt materials are crushed, ground and pretreated to increase their leaching rate.

[0024] Acid leaching treatment: Take a certain mass of pretreated high-iron copper-cobalt material, add water to slurry according to a certain liquid-solid ratio, start stirring, add concentrated sulfuric acid, and use the high heat generated by the concentrated sulfuric acid dissolved in water to quickly raise the leaching temperature to high temperature. React at high temperature for about 2 hours, then add a certain amount of ammonium bifluoride, and react for another hour. At the same time, take a certain amount of sodium chlorate to make a solution, keep the leaching temperature above 90 degrees, continue to react for 1 hour after the addition is completed, and measure the PH value at about 2.4, then filter and wash the residue.

[0025] In the pretreatment, 50 g of cobalt material was taken and 350 ml of water (liquid-to-solid volume ratio = 7:1) was added for slurrying;

[0026] According to the amount of dissolved copper and cobalt, the theoretical amount of concentrated sulfuric acid that needs to be added is calculated. A total of 20 ml of concentrated sulfuric acid is added and reacted for 2 hours. As the amount of sulfuric acid increases, the cobalt leaching rate does not change much, while the copper leaching rate increases. When the theoretical amount of sulfuric acid is increased, the copper leaching rate tends to be flat. Continuing to increase the amount of sulfuric acid, the copper leaching rate decreases slightly.

[0027] Experiment 1: This experiment is different from the above example in that the amount of concentrated sulfuric acid used is as shown in the following table:

[0028]

[0029] From the table above, we can see the effect of sulfuric acid dosage on the leaching rate of valuable metals cobalt and copper. The dosage of sulfuric acid is 1.1 times the theoretical amount (20ml, 98%), which is more reasonable.

[0030] Then 4 g of ammonium bifluoride was added and the reaction was carried out for 1 hour. As the amount of ammonium bifluoride increased, the cobalt leaching rate decreased slightly, while the copper leaching rate increased slightly.

[0031] Experiment 2: This experiment is different from the above example in that the amount of ammonium bifluoride used is changed as shown in the following table:

[0032]

[0033]

[0034] From the table above, we can see the effect of the amount of ammonium fluoride on the leaching rate of valuable metals cobalt and copper. Taking all factors into consideration, the optimal amount of ammonium bifluoride is 4g.

[0035] Then add 40g of sodium chlorate and 40ml of water to prepare a solution, keep the temperature above 90 degrees for 1 hour, with the increase of sodium chlorate dosage, the cobalt leaching rate does not change much, while the copper leaching rate changes greatly. When the sodium chlorate dosage is 0.78 times the theoretical amount, the copper leaching rate tends to be stable.

[0036] Experiment 3: This experiment is different from the above embodiment in that the amount of sodium chlorate used is changed as shown in the following table:

[0037]

[0038] From the above table, we can see the effect of ammonium fluoride dosage on the leaching rate of valuable metals cobalt and copper. Since the addition of sodium chlorate will bring in chloride ions, the optimal dosage is when the copper leaching rate just tends to be stable and the chloride ions are relatively minimal. Therefore, the optimal dosage of the oxidant is 0.78 times the theoretical dosage (the theoretical dosage is 51g sodium chlorate, which can be inferred from the Journal of Central South University (Natural Science Edition) "Oxidative Acid Leaching of Refractory Copper-Cobalt Alloys").

[0039] The test results show that for 50g of high-iron copper-cobalt material, when the liquid-solid mass volume ratio is about 1:7, the temperature is 90 to 95 degrees, the amount of sulfuric acid is 20ml (98%), 4g of ammonium bifluoride, 40g of sodium chlorate, and the reaction conditions are 2h, after filtering, by washing the filter residue, the leaching filter of cobalt, copper and iron is obtained as follows:

[0040] Co(%) With(%) Fe(%) 92.44 93.85 0

[0041] Conclusion: Leaching copper and cobalt materials with sulfuric acid, adding ammonium bifluoride as an additive and sodium chlorate as an oxidant can significantly increase the leaching rate of cobalt and copper, while most of the iron remains in the slag. This method is simple to operate, has a short process and a high metal recovery rate.

[0042] The embodiments of the present invention are given for the purpose of illustration and description, and are not intended to be exhaustive or to limit the invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.

Claims

1. A method for leaching copper and cobalt from a high-iron copper and cobalt material, characterized in that: The following steps are involved: 1) Pretreatment: crushing and grinding the high iron, copper and cobalt raw materials; 2) Dissolving; taking the pretreated high iron copper cobalt material, adding water to slurry and stirring; 3) Acid leaching treatment: add concentrated sulfuric acid to the stirred solution, heat it in water and react for 1-3 hours, then add ammonium bifluoride and react for 0.5-1.5 hours, and at the same time take sodium chlorate solution and add it dropwise to the reaction solution to continue the reaction; 4) Filtration; the solution after the reaction was filtered when the pH value was 2.2-2.6 after 1 hour, and the filter residue was washed.

2. A method for leaching copper and cobalt from a high-iron copper and cobalt material as claimed in claim 1, characterized in that: The volume ratio of the cobalt material to water in the water slurry of step 2 is 7:

1.

3. A method for leaching copper and cobalt from a high-iron copper and cobalt material as claimed in claim 1, characterized in that: In step 3, concentrated sulfuric acid is reacted for 2 hours, and ammonium bifluoride is added and reacted for 1 hour.

4. A method for leaching copper and cobalt from a high-iron copper and cobalt material as claimed in claim 1, characterized in that: Filter when the pH value in step 4 is 2.

4.

5. A method for leaching copper and cobalt from a high-iron copper and cobalt material as claimed in claim 1, characterized in that: Taking 98% concentration sulfuric acid solution as an example, the ratio of high iron, copper and cobalt raw materials to concentrated sulfuric acid is 1g: 0.36ml-0.43ml; the ratio of high iron, copper and cobalt raw materials to ammonium bifluoride is 25g: 1g-3g; the ratio of high iron, copper and cobalt raw materials to sodium chlorate is 50g: 33g-60g.

6. A method for leaching copper and cobalt from a high-iron copper and cobalt material as claimed in claim 5, characterized in that: The usage ratio of high iron copper cobalt raw material to concentrated sulfuric acid, ammonium bifluoride and sodium chlorate is 50g:20ml:4g:40g.