Forming method of amorphous alloy elastic element for mechanical arm
By using amorphous alloy materials for superplastic molding, the problem of insufficient strength and toughness of the elastic element material of the robot arm is solved, the quality and life of the elastic element is improved, the process is simplified and the cost is reduced.
Patent Information
- Application Number
- CN202411193173.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing robotic arm elastic element materials have shortcomings in terms of strength, toughness and elasticity, and it is difficult to meet the needs of high strength, high toughness and high elasticity.
Amorphous alloy is used as raw material, and elastic components are prepared by heating to melt, refining, cooling to supercooled liquid and superplastic molding, combined with rapid cooling technology to prepare elastic components to improve their mechanical properties and processing properties.
It significantly improves the quality of the elastic components of the robot arm and the product qualification rate, provides better energy absorption, longer service life and stronger wear resistance, simplifies the molding process and reduces production costs.
Smart Images

Figure CN119082537A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mechanical arm manufacturing and relates to a molding method of an amorphous alloy elastic element for a mechanical arm. Background Art
[0002] The robotic arm is a key component of the humanoid robot. The elastic element in it acts as a buffer by storing elastic energy, which requires the material to have high strength, high toughness and high elasticity. Amorphous alloy is an advanced metal material. Its microstructure is different from that of traditional crystalline materials. The atomic arrangement structure has the characteristics of long-range disorder and short-range order. Compared with traditional crystalline alloys, it has a series of unique mechanical, physical and chemical properties, such as high strength, high toughness, high elasticity and high hardness, and is an ideal material for preparing elastic elements of robotic arms. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a forming method of amorphous alloy elastic elements for robotic arms. The forming method selects amorphous alloys with excellent mechanical properties and processing properties as raw materials, and combines superplastic forming to effectively improve the quality of elastic elements for robotic arms and the product qualification rate.
[0004] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0005] The present invention provides a method for forming an amorphous alloy elastic element for a mechanical arm, the method comprising:
[0006] The raw materials of the amorphous alloy are heated until they are completely melted, and then refined to obtain an amorphous alloy melt;
[0007] Cooling the amorphous alloy melt to a supercooled liquid temperature range to obtain a supercooled liquid of the amorphous alloy;
[0008] Performing superplastic forming on the supercooled liquid to obtain an elastic element blank;
[0009] The elastic element blank is rapidly cooled to a temperature below the glass transition temperature of the amorphous alloy and then removed from the mold, and then cooled to room temperature to obtain the elastic element.
[0010] As a preferred technical solution of the present invention, the composition of the amorphous alloy is Zr x Cu a Ni b Al c Ti d Re y , Re is a rare earth element;
[0011] Wherein, a, b, c, d, x and y are all atomic percentages, and the value ranges of a, b, c, d, x and y are: 0≤a≤0.3, 0≤b≤0.3, 0≤c≤0.15, 0≤d≤0.05, 0≤ <y≤0.05;x=1-a-b-c-d-y。
[0012] The value of a can be 0, 0.1, 0.2 or 0.3, etc., the value of b can be 0, 0.1, 0.2 or 0.3, etc., the value of c can be 0, 0.05, 0.10 or 0.15, etc., the value of d can be 0, 0.01, 0.02, 0.03, 0.04 or 0.05, etc., the value of y can be 0.01, 0.02, 0.03, 0.04 or 0.05, etc., but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0013] As a preferred technical solution of the present invention, the rare earth element includes any one of Ce, La, Y, Dy, Gd or Er, or a combination of at least two of them.
[0014] As a preferred technical solution of the present invention, the mechanical properties of the zirconium-based amorphous alloy are: yield strength ≥ 1600Mpa, fracture toughness ≥ 130Mpa·m 1 / 2 , elastic limit ≥2%.
[0015] As a preferred technical solution of the present invention, refining is carried out in a high-frequency or medium-frequency induction furnace.
[0016] As a preferred technical solution of the present invention, after refining, the amorphous alloy melt is subjected to a heat preservation treatment to homogenize the composition.
[0017] As a preferred technical solution of the present invention, the temperature range T of the supercooled liquid is T g <T<T m , the T g is the glass transition temperature of the zirconium-based amorphous alloy, T m is the melting point of the zirconium-based amorphous alloy.
[0018] As a preferred technical solution of the present invention, the superplastic forming method includes causing the supercooled liquid to generate thixotropic flow under the action of an electromagnetic driving force, and completing superplastic forming under the action of pressure generated by the electromagnetic driving force.
[0019] As a preferred technical solution of the present invention, the rapid cooling method includes forced convection cooling.
[0020] As a preferred technical solution of the present invention, the forming method of the amorphous alloy elastic element for a robotic arm includes:
[0021] The raw materials of the amorphous alloy are heated until they are completely melted, and refined in a high-frequency or medium-frequency induction furnace to obtain an amorphous alloy melt;
[0022] After refining, the amorphous alloy melt is subjected to heat preservation treatment to homogenize the composition;
[0023] The amorphous alloy melt is cooled to a supercooled liquid temperature range, and the supercooled liquid temperature range is T g <T<T m , obtaining a supercooled liquid of the amorphous alloy;
[0024] The composition of amorphous alloy is Zr x Cu a Ni b Al c Ti d Re y , Re is a rare earth element; wherein a, b, c, d and y are all atomic percentages, and the value ranges of a, b, c, d, x and y are: 0≤a≤0.3, 0≤b≤0.3, 0≤c≤0.15, 0≤d≤0.05, 0 <y≤0.05;x=1-a-b-c-d-y;
[0025] The supercooled liquid is caused to flow thixotropically under the action of electromagnetic driving force, and superplastic forming is completed under the action of pressure generated by the electromagnetic driving force to obtain an elastic element blank;
[0026] The elastic element blank is subjected to forced convection cooling until the temperature is below the glass transition temperature of the amorphous alloy, and then removed from the mold, and naturally cooled to room temperature to obtain the elastic element.
[0027] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0028] The present invention provides a forming method of an amorphous alloy elastic element for a robot arm. The forming method uses an amorphous alloy with excellent mechanical properties and processing properties as a raw material and combines it with superplastic forming to effectively improve the quality of the elastic element for the robot arm and the product qualification rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic flow chart of a method for forming an amorphous alloy elastic element for a robot arm provided in a specific embodiment of the present invention.
[0030] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0032] A specific embodiment of the present invention provides a method for forming an amorphous alloy elastic element for a robotic arm, the method comprising:
[0033] The raw materials of the amorphous alloy are heated until they are completely melted, and then refined to obtain an amorphous alloy melt;
[0034] Cooling the amorphous alloy melt to a supercooled liquid temperature range to obtain a supercooled liquid of the amorphous alloy;
[0035] Performing superplastic forming on the supercooled liquid to obtain an elastic element blank;
[0036] The elastic element blank is rapidly cooled to a temperature below the glass transition temperature of the amorphous alloy and then removed from the mold, and then cooled to room temperature to obtain the elastic element.
[0037] Amorphous alloy is an advanced metal material. Its microstructure is different from that of traditional crystalline materials. The atomic arrangement structure has the characteristics of long-range disorder and short-range order. Compared with traditional crystalline alloys, it has a series of unique mechanical, physical and chemical properties, such as high strength, high elasticity, high hardness and other excellent properties. Compared with traditional alloy elastic elements, the elastic elements prepared by this process have better energy absorption effect, longer life, and stronger wear resistance. By heating the amorphous alloy raw materials to above the melting temperature to form a melt, refining and homogenizing, cooling to the supercooled liquid range, and then superplastic forming, the elastic properties of the elastic element are improved, while the forming process is simplified, the production efficiency is improved, and the production cost is reduced.
[0038] In a specific embodiment of the present invention, a, b, c, d, x and y in the composition of the amorphous alloy represent atomic percentages.
[0039] In a specific embodiment of the present invention, sponge zirconium particles, sponge titanium particles, granular yttrium, electrolytic copper, electrolytic nickel and electrolytic aluminum are selected, and a vacuum arc melting process can be used to melt the alloy material so that the melt obtains a sufficiently high superheat to ensure that all components are melted.
[0040] In a specific embodiment of the present invention, the raw materials are added into a vacuum arc furnace and then evacuated, and then a protective gas, such as argon, is introduced.
[0041] In one embodiment of the present invention, all components are melted and transferred to a high frequency or medium frequency induction furnace for further refining to homogenize the composition and temperature of the melt.
[0042] In a specific embodiment of the present invention, the melt can be kept warm in a heat preservation device, such as a heat preservation bag, to store the melt while further homogenizing the composition and temperature of the melt.
[0043] In a specific embodiment of the present invention, the refining temperature and time can be specifically selected according to the materials and their proportions, and are not further limited herein.
[0044] In a specific embodiment of the present invention, electromagnetic force can be used as a driving force to cause rapid convection of the melt, and the melt is transferred from the high-frequency or medium-frequency induction furnace or the heat preservation device to the heat exchange device for cooling the melt. The advantage of electromagnetic drive is that it does not contact the melt and is pollution-free.
[0045] In a specific embodiment of the present invention, the heat exchange device may be an enhanced convection heat exchanger, which cools the temperature of the melt to a supercooling temperature range to form a supercooling temperature.
[0046] In a specific embodiment of the present invention, a heat preservation device may be provided after the heat exchange device for heat preservation and storage of the supercooled liquid.
[0047] In one embodiment of the present invention, the glass transition temperature T of the amorphous alloy may be measured by DSC before forming. g , crystallization temperature T x , melting point T m Tests are performed to determine the subcooling temperature range.
[0048] In a specific embodiment of the present invention, the superplastic forming method includes: under the action of electromagnetic driving force, supercooled liquid generates thixotropic flow; under the action of pressure generated by the electromagnetic driving force, superplastic forming of the robot arm is completed.
[0049] In one specific embodiment of the present invention, the rapid cooling method includes: providing a cooling channel in the injection mold and using a coolant with strong cooling capacity for forced convection cooling. The coolant with strong cooling capacity can be specifically selected according to the properties of the coolant and the cooling needs, and is not further limited here.
[0050] In a specific embodiment of the present invention, the cooling channel and high thermal conductivity mold material of the injection mold can be selected according to the thermophysical parameters of different mold materials; considering that the temperature of the supercooled liquid is much lower than the melting point, materials with relatively large heat transfer coefficients, such as brass (H06 C21000 and H03 C21000) and beryllium copper (TF00C17500 copper and TF00C17510 coppe) can be selected to manufacture the injection mold.
[0051] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0052] Example 1
[0053] This embodiment provides a method for forming an amorphous alloy elastic element for a robot arm, and the process is as follows: Figure 1 As shown, the molding method includes:
[0054] Sponge Zr particles (purity 99.5%), electrolytic copper (purity 99.9%), electrolytic aluminum (purity 99.9%), and sponge titanium (purity 99.5%) were placed in a vacuum furnace according to atomic percentage and evacuated to 1×10 -3 After 1000 Pa, high-purity argon gas is introduced, and the mixture is heated to be completely melted in an argon atmosphere, and refined in a medium-frequency induction furnace to obtain an amorphous alloy melt;
[0055] After refining, the amorphous alloy melt is placed in a heat preservation bag for heat preservation treatment to further homogenize the composition;
[0056] The outlet of the insulation bag is equipped with an electromagnetic drive pump, which generates a driving force to make the melt convect quickly, and sends the amorphous alloy melt to the enhanced convection heat exchanger to cool it to the supercooled liquid temperature range. The temperature range of the supercooled liquid is T g <T<T m , obtaining a supercooled liquid of the amorphous alloy;
[0057] The supercooled liquid is caused to flow thixotropically under the action of electromagnetic driving force, and superplastic forming is completed under the action of pressure generated by the electromagnetic driving force to obtain an elastic element blank;
[0058] The elastic element blank is subjected to forced convection cooling to the glass transition temperature T of the amorphous alloy. g The elastic element is then removed from the mold and cooled to room temperature to obtain the elastic element.
[0059] The composition of amorphous alloy is Zr 0.609 Cu 0.25 Al 0.12 Ti 0.02 Y 0.001 , DSC was used to measure the glass transition temperature T of non-gold alloys before molding g , crystallization temperature T x , melting point T m .
[0060] Example 2
[0061] This embodiment provides a method for forming an amorphous alloy elastic element for a robot arm. In addition to the composition of the amorphous alloy being Zr 0.577 Cu 0.28 Al 0.12 Ti 0.02 Y 0.003 Except for this, the other conditions are the same as those in Example 1.
[0062] Example 3
[0063] This embodiment provides a method for forming an amorphous alloy elastic element for a robot arm. In addition to the composition of the amorphous alloy being Zr 0.615 Cu 0.26 Al 0.10 Ti 0.02 Y 0.005 Except for this, the other conditions are the same as those in Example 1.
[0064] Example 4
[0065] This embodiment provides a method for forming an amorphous alloy elastic element for a robot arm. In addition to the composition of the amorphous alloy being Zr 0.599 Cu 0.27 Al 0.08 Ti 0.05 Y 0.001 Except for this, the other conditions are the same as those in Example 1.
[0066] Example 5
[0067] This embodiment provides a method for forming an amorphous alloy elastic element for a robot arm. In addition to the composition of the amorphous alloy being Zr 0.615 Cu 0.23 Al 0.10 Ti 0.05 Y 0.005 Except for this, the other conditions are the same as those in Example 1.
[0068] The amorphous alloy elastic element for a robot arm prepared by the molding method provided in Examples 1-5 has better elastic properties and longer service life than the elastic element for a robot arm prepared by the conventional method. In addition, compared with the original elastic element preparation process, the process has a shorter preparation process, does not rely on precision machining machines, and has lower costs. Overall, it has better economic value.
[0069] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0070] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0071] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0072] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for forming an amorphous alloy elastic element for a robotic arm, characterized in that: The molding method comprises: The raw materials of the amorphous alloy are heated until they are completely melted, and then refined to obtain an amorphous alloy melt; Cooling the amorphous alloy melt to a supercooled liquid temperature range to obtain a supercooled liquid of the amorphous alloy; Performing superplastic forming on the supercooled liquid to obtain an elastic element blank; The elastic element blank is rapidly cooled to a temperature below the glass transition temperature of the amorphous alloy, removed from the mold, and cooled to room temperature to obtain the elastic element.
2. The zirconium-based amorphous alloy according to claim 1, characterized in that: The composition of the amorphous alloy is Zr x Cu a Ni b Al c Ti d Re y , Re is a rare earth element; Wherein, a, b, c, d, x and y are all atomic percentages, and the value ranges of a, b, c, d, x and y are: 0≤a≤0.3, 0≤b≤0.3, 0≤c≤0.15, 0≤d≤0.05, 0≤ <y≤0.05;x=1-a-b-c-d-y。 3. The zirconium-based amorphous alloy according to claim 2, characterized in that: The rare earth element includes any one of Ce, La, Y, Dy, Gd or Er, or a combination of at least two of them.
4. The zirconium-based amorphous alloy according to claim 2, characterized in that: The mechanical properties of the zirconium-based amorphous alloy are: yield strength ≥ 1600Mpa, fracture toughness ≥ 130Mpa·m 1 / 2 , elastic limit ≥2%.
5. The molding method according to claim 1, characterized in that: The refining is carried out in a high frequency or medium frequency induction furnace.
6. The molding method according to claim 1, characterized in that: After the refining, the amorphous alloy melt is subjected to a heat preservation treatment to make the composition uniform.
7. The molding method according to claim 1, characterized in that: The temperature range of the supercooled liquid is T g <T<T m , the T g is the glass transition temperature of the amorphous alloy, T m is the melting point of the zirconium-based amorphous alloy.
8. The molding method according to claim 1, characterized in that: The superplastic forming method comprises causing the supercooled liquid to generate thixotropic flow under the action of an electromagnetic driving force, and completing superplastic forming under the action of pressure generated by the electromagnetic driving force.
9. The molding method according to claim 1, characterized in that: The rapid cooling method includes forced convection cooling.
10. The molding method according to any one of claims 1 to 9, characterized in that: The molding method comprises: The raw material of the amorphous alloy is heated until it is completely melted, and refined in a high-frequency or medium-frequency induction furnace to obtain an amorphous alloy melt; After the refining, the amorphous alloy melt is subjected to a heat preservation treatment to homogenize the composition; The amorphous alloy melt is cooled to a supercooled liquid temperature range, wherein the supercooled liquid temperature range T is T g <T<T m , obtaining a supercooled liquid of the amorphous alloy; The composition of the amorphous alloy is Zr x Cu a Ni b Al c Ti d Re y , Re is a rare earth element; wherein a, b, c, d and y are all atomic percentages, and the value ranges of a, b, c, d, x and y are: 0≤a≤0.3, 0≤b≤0.3, 0≤c≤0.15, 0≤d≤0.05, 0 <y≤0.05;x=1-a-b-c-d-y; The supercooled liquid is caused to flow thixotropically under the action of an electromagnetic driving force, and is superplastically formed under the action of pressure generated by the electromagnetic driving force to obtain an elastic element blank; The elastic element blank is subjected to forced convection cooling until the temperature is below the glass transition temperature of the amorphous alloy, and then removed from the mold, and cooled to room temperature to obtain the elastic element.