Fatigue-resistant high-carbon steel wire rod and manufacturing method thereof
By optimizing the alloy composition and process flow of high-carbon steel, the shortcomings of high-carbon steel wires in torsional fatigue performance have been solved, and the torsional strength and fatigue life have been significantly improved, which is suitable for high-end products in the machinery industry.
Patent Information
- Application Number
- CN202310659994.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The prior art lacks research on torsional fatigue properties in high-carbon steel materials, especially in terms of torsional fatigue resistance of wires, and the prior art solutions are mainly applicable to plates but not wires.
By optimizing the alloy composition design of high-carbon steel, combined with specific process flows such as smelting, rolling, Steyrmo fan cooling, spherical annealing and drawing, the content and tissue structure of chemical elements are controlled to obtain excellent resistance to torsion fractures. Performance high-carbon steel wire.
It has achieved the torsional strength of high-carbon steel wires exceeding 1700MPa and torsional fatigue life exceeding 10,000 times. It is suitable for high-end products in the machinery industry, making up for the gap in the domestic market and improving the processing level.
Smart Images

Figure BDA0004268363900000051 
Figure BDA0004268363900000061 
Figure BDA0004268363900000062
Abstract
Description
Technical Field
[0001] The invention relates to a steel material and a preparation method thereof, and in particular to a wire material and a preparation method thereof. Background Art
[0002] Hardness and fatigue performance are important indicators for judging the quality of steel materials. Generally speaking, the higher the hardness, the better the wear resistance of the material and the longer the product life. On the other hand, many machine tool parts, in addition to high hardness, also have certain requirements for torsional fatigue resistance due to long-term torsional shear forces.
[0003] At present, the research on torsional fatigue performance of steel materials is mainly concentrated in the field of medium and low carbon steel, while there is less research on high carbon steel.
[0004] For example, the Chinese patent document with publication number CN 110760748 A, publication date February 7, 2020, and titled “A spring steel with excellent fatigue life and its manufacturing method” discloses a spring steel with excellent fatigue life and its manufacturing method, the alloy composition of which is: C: 0.52-0.62%, Si: 1.20-1.45%, Mn: 0.25-0.75%, Cr: 0.30-0.80%, V: 0.01-0.15%, Nb: 0.001-0.05%, N: 0.001-0.009%, O: 0.0005-0.0040%, P≤0.015%, S≤0.015%, Al≤0.0045%, and satisfies 0.02≤(2Nb+V) / (20N+C)≤0.40. However, the carbon content of this technical solution is low and does not involve torsional performance.
[0005] For another example, the Chinese patent document with publication number CN107419175A, publication date December 1, 2017, and titled "Economical tool steel with good fatigue life and production method thereof" discloses a method for producing economical tool steel with good fatigue life, wherein the alloy composition of the material is: C: 0.75-1.00%, Si: 0.15-0.35%, Mn: 0.50-1.20%, Cr: 0.30-1.10%, V: 0.05-0.20%, Alt≤0.040%, P≤0.020%, S≤0.010%, N≤0.006%, and a uniform granular pearlite structure is obtained after hot rolling annealing, and a fine tempered martensite structure is obtained after quenching and tempering. However, this technical solution is only applicable to plates, not wires. Summary of the invention
[0006] One of the purposes of the present invention is to provide a fatigue-resistant high-carbon steel wire, which is based on high-carbon steel, optimizes the alloy composition design, and realizes organizational regulation in conjunction with a specific process, thereby obtaining excellent torsional fracture resistance, which can be effectively applied to high-end products in the machinery industry.
[0007] In order to achieve the above object, the present invention provides a fatigue-resistant high-carbon steel wire, which contains Fe and inevitable impurities, and further contains the following chemical elements in the following mass percentages:
[0008] C: 0.60~0.90%, Si: 1.00~3.00%, Mn: 0.45~1.00%, Cr: 0.45~1.00%, Ni: 0.10~0.30%, Ti: 0.01~0.20%, Cu: 0.05~0.50%, (La+Ce): 0.01~0.10%.
[0009] Furthermore, the present invention also provides a fatigue-resistant high-carbon steel wire, the mass percentage of each chemical element of which is:
[0010] C: 0.60~0.90%, Si: 1.00~3.00%, Mn: 0.45~1.00%, Cr: 0.45~1.00%, Ni: 0.10~0.30%, Ti: 0.01~0.20%, Cu: 0.05~0.50%, (La+Ce): 0.01~0.10%; the balance is Fe and other inevitable impurities.
[0011] In the fatigue-resistant high-carbon steel wire of the present invention, the design principles of each chemical element are specifically described as follows:
[0012] C: In the fatigue-resistant high-carbon steel wire described in the present invention, C is the most important element. On the one hand, C can play a role in solid solution strengthening in steel, and on the other hand, C can form various carbides. It should be noted that when the C content in the steel is too low, it is difficult to ensure the hardness and wear resistance of the steel; and when the C content in the steel is too high, it will have an adverse effect on the toughness of the steel, making segregation difficult to control, increasing the difficulty of smelting and rolling, and easily producing abnormal structures such as network carbides. Taking into account the influence of the C element on the performance of the fatigue-resistant high-carbon steel wire in the present technical solution, in the fatigue-resistant high-carbon steel wire described in the present invention, the mass percentage of C is controlled between 0.60 and 0.90%.
[0013] Si: In the fatigue-resistant high-carbon steel wire described in the present invention, Si is a non-carbide-forming element. The Si element has a strong solid solution strengthening effect in steel, which can effectively improve the hardness of tool steel. However, it should be noted that the Si content in the steel should not be too high. When the Si content in the steel is too high, the toughness of the steel will be reduced. Therefore, in the fatigue-resistant high-carbon steel wire described in the present invention, the mass percentage of the Si element is controlled between 1.00 and 3.00%.
[0014] Mn: In the fatigue-resistant high-carbon steel wire of the present invention, the Mn element can effectively improve the hardenability of the steel, improve the stability of austenite, delay the transformation of pearlite, and improve the impact toughness. Considering the requirements of the fatigue-resistant high-carbon steel wire of the present invention for hardenability, the mass percentage of the Mn element is controlled between 0.45 and 1.00%.
[0015] Cr: In the fatigue-resistant high-carbon steel wire of the present invention, the Cr element can effectively improve the hardenability, hardenability and tempering stability of the steel. As a carbide-forming element, Cr can form carbides with C in steel, and can also be dissolved in ferrite to play a strengthening role. Therefore, considering its strengthening effect and production cost, in the fatigue-resistant high-carbon steel wire of the present invention, the mass percentage of the Cr element is controlled between 0.45 and 1.00%.
[0016] Ni: In the fatigue-resistant high-carbon steel wire of the present invention, the role of Ni in the steel is mainly to reduce the low-temperature brittle transition temperature, which can improve the strength of the steel without significantly reducing the toughness, while improving the corrosion resistance of the steel, reducing the notch sensitivity of the steel and improving the fatigue performance. Considering the beneficial effects and costs of Ni, the mass percentage of Ni in the fatigue-resistant high-carbon steel wire of the present invention can be controlled between 0.10 and 0.30%.
[0017] Ti: In the fatigue-resistant high-carbon steel wire of the present invention, the Ti element can be added to the steel as a microalloying element. As a strong carbonitride-forming element, it mainly plays a role in refining the grains, improving the hardness of the steel and also having a good effect on toughness. Therefore, in the fatigue-resistant high-carbon steel wire of the present invention, the mass percentage of Ti can be controlled to be 0.01-0.20%.
[0018] Cu: In the fatigue-resistant high-carbon steel wire described in the present invention, the Cu element can improve the corrosion resistance of the steel, but too high a content thereof will lead to a decrease in hot workability and a decrease in the manufacturability of the steel. Therefore, in the fatigue-resistant high-carbon steel wire described in the present invention, the mass percentage of Cu can be controlled between 0.05 and 0.50%.
[0019] La, Ce: In the fatigue-resistant high-carbon steel wire described in the present invention, La and Ce have a purifying and obvious modification effect. The cleanliness of steel is constantly improving, and the micro-alloying effect of rare earth elements is becoming increasingly prominent. Rare earth micro-alloying includes solid solution strengthening of trace rare earth elements, interaction between rare earth elements and other solute elements and compounds, the existence state, size, form and distribution of rare earth elements, especially the segregation at grain boundaries and the influence of rare earth on the surface and matrix structure of steel. In the fatigue-resistant high-carbon steel wire described in the present invention, the mass percentage of (La+Ce) can be controlled to 0.01-0.10%.
[0020] Furthermore, among other inevitable impurities in the fatigue-resistant high carbon steel wire of the present invention: P≤0.015%, S≤0.015%.
[0021] Under the condition that technical conditions permit, in order to obtain steel with better performance and better quality, the content of impurity elements in fatigue-resistant high-carbon steel wire should be reduced as much as possible. The inevitable impurities in the present invention are mainly P and S. Impurity elements P and S are prone to segregation at grain boundaries, reducing the toughness of steel and having a great impact on the cold working performance of steel. Based on this, in some embodiments, P≤0.015% and S≤0.015% can be controlled.
[0022] Furthermore, in the fatigue-resistant high carbon steel wire rod described in the present invention, its hot-rolled microstructure is upper bainite+martensite.
[0023] Furthermore, in the fatigue-resistant high carbon steel wire rod of the present invention, the microstructure thereof after quenching and tempering and isothermal heat treatment is lower bainite.
[0024] Furthermore, the fatigue-resistant high-carbon steel wire described in the present invention has a torsional strength greater than 1700 MPa and a torsional fatigue life greater than 10,000 times.
[0025] Another object of the present invention is to provide a method for manufacturing fatigue-resistant high-carbon steel wire, which adopts a relatively simple processing technology to obtain a wire with excellent fatigue resistance.
[0026] Based on the above purpose, the present invention also provides a method for manufacturing a fatigue-resistant high-carbon steel wire, which comprises the steps of:
[0027] smelting and casting;
[0028] Rolled into wire rod;
[0029] Stelmore fan cooling: Stelmore air cooling line is used to control the wire rod cooling rate to 0.3~2℃ / s;
[0030] Spheroidizing annealing;
[0031] Pull.
[0032] The manufacturing method of the fatigue-resistant high-carbon steel wire rod of the present invention can obtain a wire rod with a specification of φ5.5-28mm by smelting, casting, rolling into wire rod and controlling cooling technology in combination with alloy component design.
[0033] Among them, after rolling into wire rod, Stelmore fan cooling adopts slow cooling measures to control the cooling rate of wire rod to 0.3~2℃ / s.
[0034] In some embodiments, the specific operation may be: through the Stelmore air cooling line, all fans are turned off and covered with a heat preservation cover.
[0035] Furthermore, in the manufacturing method of the present invention, in the Stelmor blower cooling step, the wire rod is kept in the heat preservation cover for 600 to 800 seconds, and the temperature out of the heat preservation cover is 540 to 780° C. At this time, the hot-rolled structure of the wire rod is upper bainite + martensite.
[0036] Afterwards, fatigue-resistant high-carbon steel wire can be obtained through spheroidizing annealing and drawing processes.
[0037] Furthermore, in the manufacturing method described in the present invention, after the drawing step, it also includes: tempering isothermal heat treatment: heating the wire to an austenitizing temperature of 820-960°C, keeping it warm for 0.5-1h, and then cooling it to an isothermal temperature in a salt bath for isothermal treatment, wherein the isothermal temperature is 200-400°C and the isothermal time is 2-5h.
[0038] Furthermore, in the manufacturing method of the present invention, the cooling rate in the salt bath is 10 to 50° C. / s.
[0039] Through subsequent tempering and isothermal heat treatment, fatigue-resistant high-carbon steel wire with torsional strength > 1700 MPa and torsional fatigue life > 10,000 times can be obtained.
[0040] The fatigue-resistant high carbon steel wire of the present invention has the following advantages and beneficial effects:
[0041] The fatigue-resistant high-carbon steel wire described in the present invention can obtain excellent fatigue resistance based on high-carbon steel, and can achieve torsional strength > 1700MPa and torsional fatigue life > 10,000 times, so it can be effectively applied to high-end products in the machinery industry, fill the gap in the domestic market in this field, and improve the processing level of the machinery industry. DETAILED DESCRIPTION
[0042] The fatigue-resistant high-carbon steel wire and the preparation method thereof described in the present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.
[0043] The fatigue-resistant high carbon steel wires of Examples 1-8 were all prepared by the following steps:
[0044] (1) Smelting and casting.
[0045] (2) Rolling into wire rod: The wire rod specification is φ5.5~28mm, and the chemical composition is shown in Table 1.
[0046] (3) Stelmore fan cooling: Turn off all fans and cover the insulation cover to control the wire rod cooling rate to 0.3-2°C / s; control the wire rod time in the insulation cover to 600-800s, and the temperature out of the insulation cover to 540-780°C.
[0047] (4) Offline spheroidizing annealing: Heat the wire rod to 760-840℃ with the furnace, keep it at this temperature for 4-6h, cool it to 710-750℃ at a rate of 10-50℃ / h, keep it at this temperature for 4-7h, and then cool it to below 600℃ at a rate of 10-50℃ / h before taking it out of the furnace.
[0048] (5) Pulling.
[0049] (6) Tempering isothermal heat treatment: Heat the wire to the austenitizing temperature of 820-960°C, keep it warm for 0.5-1h, then quickly put it into a salt bath and cool it to the isothermal temperature for isothermal treatment. The isothermal temperature is 200-400°C and the isothermal time is 2-5h.
[0050] In some embodiments, the cooling rate of the wire in the salt bath is 10-50° C. / s.
[0051] Table 1 lists the mass percentages of the chemical elements of the fatigue-resistant high carbon steel wires of Examples 1-8.
[0052] Table 1. (wt%, the balance is Fe and other inevitable impurities except P and S)
[0053]
[0054]
[0055] Table 2 lists the specific process parameters of the fatigue-resistant high carbon steel wires of Examples 1-8 in the above steps.
[0056] Table 2.
[0057]
[0058] The wire rods of Examples 1-8 were sampled in their hot rolled and tempered states, and the microstructures were analyzed using the metal microstructure inspection method (GB / T 13298-201). It was found that the microstructures in the hot rolled state were upper bainite + martensite, and the microstructures after the tempering isothermal heat treatment were lower bainite.
[0059] In addition, the fatigue-resistant high carbon steel wires of Examples 1-8 obtained through the above process steps after quenching and isothermal heat treatment were sampled and subjected to relevant performance tests. The obtained performance test results are listed in Table 3.
[0060] The specific test method is as follows: the test is carried out in accordance with the relevant provisions of GB / T 10128-2007 "Metallic Materials Room Temperature Torsion Test Method", the processing sample size is φ7mm, the total length is 150mm, the gauge length is 50mm, the torsion speed is 30° / min, and the test temperature is room temperature.
[0061] Table 3 lists the relevant performance test results of fatigue-resistant high carbon steel wires of Examples 1-8.
[0062] Table 3.
[0063]
[0064]
[0065] As shown in Table 3, the torsional strength of the wires in Examples 1-8 is all greater than 1700 MPa, and the fatigue times are all greater than 10,000 times. This shows that it not only has good torsional strength, but also has excellent fatigue resistance. Therefore, the fatigue-resistant high-carbon steel wire of the present invention has significant advantages in torsional strength and fatigue resistance, and can be effectively applied to high-end products in the machinery industry.
[0066] In addition, the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0067] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.
Claims
1. A fatigue-resistant high-carbon steel wire containing Fe and inevitable impurities, It is characterized in that It also contains the following chemical elements in the following mass percentages: C: 0.60~0.90%, Si: 1.00~3.00%, Mn: 0.45~1.00%, Cr: 0.45~1.00%, Ni: 0.10~0.30%, Ti: 0.01~0.20%, Cu: 0.05~0.50%, (La+Ce): 0.01~0.10%.
2. The fatigue-resistant high carbon steel wire according to claim 1, It is characterized in that The mass percentage of each chemical element is: C: 0.60~0.90%, Si: 1.00~3.00%, Mn: 0.45~1.00%, Cr: 0.45~1.00%, Ni: 0.10~0.30%, Ti: 0.01~0.20%, Cu: 0.05~0.50%, (La+Ce): 0.01~0.10%; The balance is Fe and other inevitable impurities.
3. The fatigue-resistant high carbon steel wire according to claim 1 or 2, It is characterized in that Among other inevitable impurities: P ≤ 0.015%, S ≤ 0.015%.
4. The fatigue-resistant high carbon steel wire according to claim 1 or 2, It is characterized in that Its hot rolled microstructure is upper bainite + martensite.
5. The fatigue-resistant high carbon steel wire according to claim 1 or 2, It is characterized in that Its microstructure after quenching and tempering and isothermal heat treatment is lower bainite.
6. The fatigue-resistant high carbon steel wire according to claim 1 or 2, It is characterized in that Its torsional strength is greater than 1700MPa and its torsional fatigue life is greater than 10,000 times.
7. The method for producing a fatigue-resistant high carbon steel wire according to any one of claims 1 to 6, It is characterized in that It includes the steps of: smelting and casting; Rolled into wire rod; Stelmore fan cooling: Stelmore air cooling line is used to control the wire rod cooling rate to 0.3~2℃ / s; Spheroidizing annealing; Pull.
8. The manufacturing method according to claim 7, It is characterized in that After the drawing step, the method further includes: tempering isothermal heat treatment: heating the wire to an austenitizing temperature of 820-960° C., keeping the temperature for 0.5-1 hour, and then cooling it to an isothermal temperature in a salt bath for isothermal treatment, wherein the isothermal temperature is 200-400° C. and the isothermal time is 2-5 hours.
9. The manufacturing method according to claim 8, It is characterized in that In the cooling step of the Stelmore blower, the time of the wire rod in the heat preservation hood is controlled to be 600-800s, and the temperature out of the heat preservation hood is 540-780°C.
10. The manufacturing method according to claim 8, It is characterized in that The cooling rate in the salt bath is 10 to 50°C / s.
Citation Information
Patent Citations
High-strength and high-toughness alloy tool steel wire rod and manufacturing method thereof
CN114318125A
Direct patenting high strength wire rod and method for producing same
CN1341155A
Production of hard steel wire rod for cold wire drawing excellent in wire drawability and fatigue characteristic
JP1995258787A
Manufacture of high strength steel excellent in fatigue characteristic
JP1999269541A