1000MPa-grade steel plate with high toughness, strain aging embrittlement resistance and excellent weldability and manufacturing method thereof
A 1000MPa grade steel plate with optimized composition and manufacturing process addresses weldability and toughness issues, ensuring high strength and resistance to strain aging embrittlement, improving safety and reducing costs in heavy-load structures.
Patent Information
- Application Number
- CN202411170289.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing high-strength steel plates face issues with low-temperature toughness, elongation, weldability, and strain aging embrittlement due to high alloy content, leading to safety hazards in heavy-load structures, and manufacturing processes are energy-intensive and costly.
A 1000MPa grade steel plate with controlled composition and manufacturing process involving controlled rolling, special tempering, and quenching to achieve high toughness, resistance to strain aging embrittlement, and excellent weldability, using elements like C, Si, Mn, Ni, Cr, Mo, V, Nb, and Ca to optimize microstructure and properties.
The steel plate achieves ultra-high strength with excellent toughness, plasticity, and weldability, reducing manufacturing costs and energy consumption, enhancing safety and stability in large steel structures.
Smart Images

Figure CN119082599A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of low-carbon high-strength low-alloy steel, in particular to a 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability and a manufacturing method thereof. Background Art
[0002] Existing high-strength steel plates with tensile strength ≥950MPa are mainly produced by offline quenching and tempering process (i.e. RQ+T); however, for steel plates with thickness ≤60mm, online quenching and tempering process (i.e. DQ+T) can also be used for production; in order to obtain ultra-high strength, the steel plate must have a sufficiently high hardenability, that is, the steel plate hardenability index DI ≥3.50×the thickness of the finished steel plate〖DI = 0.311(%C) 1 / 2 [(1 + 0.64(%Si)]×[(1 + 4.10(%Mn)]×[(1 + 0.27(%Cu)]×[(1 + 0.52(%Ni)]×[(1 + 2.33(%Cr)]×[(1 + 3.14(%Mo)]×25.4(mm)〗, in order to ensure that the steel plate has sufficiently high strength, excellent low-temperature toughness and uniform microstructure and performance along the thickness direction, it is inevitable to add a large amount of alloying elements such as Cr, Mo, Ni, Cu, V, etc. to the steel, especially the Ni content is added to more than 2.00%, resulting in high carbon equivalent and cold crack sensitivity index of the steel plate, which seriously affects the weldability of the steel plate; In addition, the surface (sub) layer of steel plates with high alloy content is prone to over-quenching, forming a coarse martensitic structure, which seriously deteriorates the low-temperature toughness and elongation of the surface (near) layer of the steel plate [Electric Power and Civil Engineering (Japanese), 1986, Vol. 201, P33; Iron and Steel, 1986, Vol. 72, S612; Iron and Steel, 1986, Vol. 72, S614; Iron and Steel, 1985, Vol. 71, S 1523; Iron and Steel, 1986, Vol.72, S615; Iron and Steel, 1986, Vol.73, S1398; Kawasaki Steel Technical Report (Japanese), 1988, Vol.20, P233; Ironmaking Research (Japanese), 1986, Vol.322, P99; CAMP-ISIJ (Japanese), 1989, Vol.3, P207; NKK Technical Report (Japanese), 19 90, Vol.133, P37; Electric Power and Civil Engineering (Japanese), 1994, Vol.249, P1; Sumitomo Metal (Japanese), 1995, Vol.47, P1; Nishiyama Memorial Technical Lecture 191-192, 2008, P162]; Low elongation and low temperature toughness are not only not conducive to the cold and hot processing performance of steel plates, but also have a great impact on the fatigue resistance, stress concentration sensitivity, crack resistance and structural stability of steel plates; when used in fatigue heavy-load structures such as pressure water pipes and volutes in hydropower projects, thermal power steam turbine generators and offshore oil production platform structures, there are great safety hazards; therefore, when large fatigue heavy-load steel structures use ultra-high strength steel, it is generally hoped that the 100 kg high-strength steel not only has excellent toughness, strong plasticity matching and weldability, but also has an elongation of more than 14% to ensure the processing performance and fatigue resistance of the steel plate.
[0003] A large number of existing patents and technical documents only explain how to achieve the strength and low-temperature toughness of the parent steel plate, but there are few descriptions on improving the welding performance of the steel plate and obtaining excellent low-temperature toughness of the HAZ in the welding heat affected zone. There is no description on how to improve the tensile strength of the steel plate while improving the tensile elongation and uniformity of mechanical properties in the thickness direction of the steel plate, and there is no indication on how to prevent the surface (sub) layer of the steel plate from being overquenched [Sho 63-93845, Sho 63-79921, Sho 60-258410, Te Pingkai 4-285119, Te Pingkai 4-308035, Ping 3-264614, Ping 2-250917, Ping 4-143246, US Patent 5798004, EP 0288054A2, Xishan Memorial Technical Lecture No. 159-160, P79~P80].
[0004] In the existing applications for 1000MPa grade quenched and tempered steel plates and their manufacturing methods (ZL201010227961.8, ZL201910566603.0), although the comprehensive mechanical properties of the steel plates have also reached a relatively high level: tensile strength ≥950MPa, yield strength ≥890MPa, -60℃ Charpy transverse impact energy (single value) ≥47J, the steel plate manufacturing technology of the invention adopts controlled rolling + offline quenching and tempering process (offline quenching + tempering); this not only has many manufacturing steps, a long manufacturing cycle, and high manufacturing costs, but also the energy consumption of the manufacturing process is relatively high (the steel plate is rolled and naturally air-cooled to room temperature, and then shot blasted and heated to the quenching temperature again), which is not conducive to energy saving and environmental protection.
[0005] Although the existing technology has also developed an online quenching and tempering + high temperature tempering process to produce 1000MPa steel plates (ZL201110071217.8, application number 202210080215.3); however, the steel plate does not involve the requirements for resistance to strain aging embrittlement. More importantly, the actual performance of the steel plate's resistance to strain aging is unstable and the data discreteness is large, which cannot meet the requirements of large hydropower stations and high-head pumped storage power stations. Summary of the invention
[0006] The purpose of the present invention is to adopt a combination of controlled rolling and special tempering technology, and on the basis of reasonable component combination design, to obtain ultra-high strength while also achieving excellent steel plate strength-toughness / strength-plasticity matching, resistance to strain aging embrittlement characteristics and weldability, and successfully solve the contradictions between the strength, plastic toughness, low-temperature toughness, resistance to strain aging embrittlement characteristics and weldability of ultra-high strength steel plates and the problem of over-quenching of the surface (sub) layer of the steel plate.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, the weight percentage of the composition elements is: C: 0.07%~0.11%, Si: ≤0.15%, Mn: 0.85%~1.10%, P: ≤0.012%, S: ≤0.0020%, Cu: 0.15%~0.45%, Ni: 1.50%~2.20%, Cr: 0.45%~0.70%, Mo: 0.35%~0.60%, V: 0.030%~0.060%, Nb: 0.010%~0.030%, Als: 0.030%~0.060%, B: ≤0.0004%, N: ≤0.0040%, O: ≤0.0030%, Ca: 0.0010%~0.0035%, The rest are Fe and other unavoidable impurities; and the contents of the above elements satisfy the following relationship at the same time: [(%Mn)+0.69(%Ni)] / (%C)≥21.5; (%C)×[(6.53(%Si)+5.17(%Als)+1.55(%Mn)+10.67(%P)+26.39(%S)+25.3(%O)]≤0.205; Ca / S is between 1.00 and 3.00 and (%Ca)×(%S) 0.18 ≤1.5×10 -3 .
[0008] Preferably, the steel plate has a tensile strength ≥950 MPa, a yield strength ≥890 MPa, a -60°C transverse impact energy ≥70 J, a -40°C aging transverse impact energy ≥70 J, and a fracture elongation δ5 ≥15%.
[0009] More preferably, the thickness of the steel plate is ≥20 mm.
[0010] A method for manufacturing a 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, for preparing the above-mentioned 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, comprises the following steps: Step 1: Smelting: According to the composition of claim 1, continuous casting is adopted, the tundish pouring superheat ΔT is controlled at 15°C to 30°C, the pulling speed is controlled at 0.5m / min to 1.0m / min, and the crystallizer liquid level fluctuation is controlled at ≤3mm; Step 2: Rolling: The first stage is ordinary rolling, the slab heating temperature is controlled at 1100℃~1170℃, the rolling reduction ratio is ≥4.0, and the rolling width ratio ζ is ≥1.4; The second stage adopts controlled rolling, with the start rolling temperature of controlled rolling ≤830℃, the rolling pass reduction rate ≥8%, the cumulative reduction rate of the non-crystallized zone with a temperature of ≤830℃ ≥50%, and the final rolling temperature of 750℃~800℃; Step 3: Cooling: After the controlled rolling is completed, the steel plate is slowly cooled. The slow cooling process is to keep the steel plate surface temperature ≥310℃ for more than 24 hours, and then the steel plate is naturally cooled to room temperature: Step 4: Quenching and tempering process: The off-line quenching and tempering process is used for production. The quenching temperature of the steel plate is dynamically adjusted according to the hardenability index of the steel plate and the Ac3 point temperature to achieve a match between the hardenability of the steel plate, the quenching temperature and the quenching roller speed; Quenching: quenching temperature is 840~870℃, quenching time in the furnace is ≥2.0H minutes, H is the thickness of the finished steel plate, and the quenching roller speed is 2.0m / min~4.0m / min; Tempering: the tempering temperature of the steel plate is 575℃~615℃, the tempering time in the furnace is ≥ the quenching time in the furnace is ≥3.0H minutes, and H is the thickness of the finished steel plate; After tempering, the steel plate is naturally cooled to room temperature.
[0011] Preferably, step one also includes: to ensure that the as-cast structure of the slab is fully crushed, the microstructure of the ultra-high strength quenched and tempered steel plate is uniform and fine, and the anisotropy of the longitudinal and transverse properties is low, the surface layer of the steel plate has a certain strain storage rate, and the total compression ratio of the steel plate, that is, the slab thickness / finished steel plate thickness is ≥4.0, and the total width ratio is ≥1.4.
[0012] Preferably, the step 2 also satisfies the following relationship: ; in, is the cumulative reduction rate without recrystallization, unit: % ζ is the rolling width ratio, unit is %; T 终轧 is the final rolling temperature, in °C; H is the thickness of the finished steel plate in mm.
[0013] Preferably, the step 4 also satisfies the following relationship: 0.31≤{[(T 淬火 )-(Ac3)]×DI} / [(V 淬火 )×ln(t 淬火 )×PT]}≤0.43; Among them, T 淬火 is the quenching and holding temperature, in °C; Ac3 is the temperature at which the austenite transformation is completed, in °C; DI is the hardenability index, in mm; V 淬火 is the roller speed of quenching, in m / min; t 淬火 is the quenching time in the furnace, in min; PT is the tempering characteristic parameter.
[0014] As a more preferred embodiment, the austenite transformation completion temperature Ac3 in step 4 also satisfies the following relationship: Ac3=910-203(%C) 0.5 +44.7(%Si)-15.2(%Ni)+31.5(%Mo)+104(%V)+13.1(%W)-[30(%Mn)+11(%Cr)+20(%Cu)-700(%P)-400(%Al)-120(%As)-400(%Ti)].
[0015] Furthermore, the hardenability index DI in step 4 also satisfies the following relationship: DI=0.367C 0.5 [(1+0.7(%Si)][(1+3.33(%Mn)][(1+0.35(%Cu)][(1+0.36(%Ni)][(1+2.1 6(%Cr)][(1+3(%Mo)][(1+1.75(%V)][(1+1.77(%Al)][(1+200(%B)]×25.4.
[0016] Furthermore, the tempering characteristic parameter PT in step 4 also satisfies the following relationship: PT=(T 回火 )[20+lg(t 回火 )]; Among them, T 回火 is the tempering temperature, in K; t 回火 Tempering time in the furnace, in minutes.
[0017] Beneficial effects of the present invention: While obtaining excellent 950MPa grade ultra-high strength quenched and tempered steel plates, the steel plates also have excellent toughness / plasticity, strain aging embrittlement resistance, and weldability, and successfully solved the contradictions and irreconcilable contradictions between the strength, plasticity, low temperature toughness, aging embrittlement resistance, and weldability of ultra-high strength steel plates, greatly improving the safety, stability, and fatigue resistance of large heavy steel structures. Good weldability saves the cost of steel component manufacturing for users, shortens the time of steel component manufacturing for users, and creates huge value for users. Therefore, this type of steel plate is not only a high value-added, green and environmentally friendly product. In addition, the invention adopts online controlled rolling + special quenching and tempering heat treatment process to give full play to the hardenability and hardenability potential of alloy elements, and the hardenability and hardenability of elements are maximized, ensuring that the steel plate has ultra-high strength, strong toughness / strong plasticity, strain aging embrittlement resistance, excellent weldability, and uniform performance along the thickness direction of the steel plate (that is, strength, toughness, plasticity and strain aging embrittlement resistance in the thickness direction basically do not change); this not only reduces the amount of alloy added to the steel plate, especially the Ni content, but also improves the weldability of the steel plate (Ceq is relatively low), especially for ultra-high strength steel plates, the sensitivity of welding cold cracking is greatly reduced, the welding preheating and post-heating temperatures are reduced, and the range of suitable welding heat input is wider, which correspondingly reduces the cost of user processing and manufacturing. In addition, a high-tech, high-value-added ultra-high strength steel plate green manufacturing technology with Chinese characteristics has been formed, which has enhanced the brand image and core competitiveness of my country's high-performance steel plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the microstructure of the newly invented steel 4 in Example 6; Figure 2 It is a table of each component in Example 3 to Example 7; Figure 3 This is a table of the conditions for the first stage of smelting and rolling in Examples 3 to 7; Figure 4 This is a table of the rolling conditions in the second stage in Examples 3 to 7; Figure 5 This is a table of the modulation process conditions in Examples 3 to 7; Figure 6 This is a table of the performance test results of each steel plate in Example 3 to Example 7. DETAILED DESCRIPTION
[0019] As follows, embodiments are further described with reference to the accompanying drawings.
[0020] As a preferred embodiment 1: to obtain an ultra-high strength steel plate with a tensile strength of ≥950MPa, a yield strength of ≥890MPa, a -60°C transverse impact energy (single value) of ≥70J, a -40°C aging transverse impact energy (single value) of ≥70J, a fracture elongation δ5 of ≥15% and excellent weldability; the composition is designed as follows: C has a great influence on the strength, low-temperature toughness, elongation, strain aging embrittlement resistance and weldability of ultra-high strength steel plates. From the perspective of improving the intrinsic plastic toughness, strain aging embrittlement resistance and weldability of ultra-high strength steel plates, it is hoped that the C content in the steel can be controlled at a lower level; however, from the perspective of hardenability, strength assurance, strength-toughness matching, microstructure control during quenching and tempering, and manufacturing cost of ultra-high strength steel plates, the C content should not be controlled too low, especially for ultra-high strength 1000MPa grade steel plates; therefore, the reasonable range of C content is 0.07% to 0.11%.
[0021] Si promotes the deoxidation of molten steel and can improve the strength of steel plates. However, for molten steel deoxidized by Al, the deoxidation effect of Si is not significant. Although Si can improve the strength of steel plates, Si promotes the coarsening of packet size, which seriously damages the low-temperature toughness, strain aging embrittlement resistance, elongation and weldability of ultra-high strength steel plates. Especially under large heat input welding conditions, Si not only promotes the formation of MA islands, but also the size of the formed MA islands is relatively large and unevenly distributed, which seriously damages the toughness of the welding heat affected zone (HAZ) and the SR performance of the welded joint. Therefore, the Si content in steel should be controlled as low as possible. Considering the economy and operability of the steelmaking process, the Si content is controlled below 0.15%.
[0022] As the most important alloying element, Mn not only improves the strength of steel plates, but also has the functions of expanding austenite phase area, reducing Ar3 point temperature, refining packet structure scale of microstructure, increasing V1 / V2 grain boundary ratio of block structure to improve plastic toughness of steel plates, and promoting the formation of low-temperature phase transformation structure martensite and bainite to improve strength of steel plates. However, Mn is easy to segregate during the solidification of molten steel, especially when the Mn content is high, which will not only make casting operation difficult, but also easily co-segregate with C, P, S, Mo, Cr and other elements. Especially when the C content in steel is high, the segregation and looseness of the center of the ingot will be aggravated, and the serious ingot will be The segregation in the central region is prone to form abnormal structures in the subsequent quenching and tempering and welding processes, resulting in low low-temperature toughness of the ultra-high strength steel plate and cracks in the welded joints; in addition, when the alloy content is high, a higher Mn content will promote the formation of coarse martensite, deteriorating the low-temperature toughness and anti-aging embrittlement characteristics of the steel plate; therefore, it is extremely necessary to select an appropriate Mn content range for ultra-high strength quenched and tempered steel plates according to the C content range. According to the steel component system of the present invention, the C content is 0.07% to 0.11% and the manufacturing process characteristics, the suitable Mn content is 0.70% to 1.10%, and when the C content is high, the Mn content is appropriately reduced, and vice versa; and when the C content is low, the Mn content is appropriately increased.
[0023] As a harmful inclusion in steel, P has a great detrimental effect on the mechanical properties of steel plates, especially low-temperature impact toughness, elongation, resistance to strain aging embrittlement, weldability and SR performance of welded joints. In theory, the lower the better; but considering the operability and cost of steelmaking, for ultra-high strength quenched and tempered steel plates that require excellent weldability, -60℃ low-temperature toughness, resistance to strain aging embrittlement and excellent strength-toughness / strength-ductility matching, the P content needs to be controlled at ≤0.012%.
[0024] As a harmful inclusion in steel, S has a great damaging effect on the low-temperature toughness of the steel plate. More importantly, S combines with Mn in the steel to form MnS inclusions. During the hot rolling process, the plasticity of MnS causes MnS to extend along the rolling direction, forming a MnS inclusion belt along the rolling direction, which seriously damages the low-temperature impact toughness, strain aging embrittlement resistance, elongation, Z-direction performance, weldability and SR performance of the steel plate. At the same time, S is also the main element that produces hot brittleness during hot rolling. In theory, the lower the better; but considering the operability of steelmaking, steelmaking cost and the principle of smooth logistics, for ultra-high strength quenched and tempered steel plates requiring excellent weldability, -60℃ low-temperature toughness, strain aging embrittlement resistance and excellent strength-toughness / strength-plasticity matching, the S content needs to be controlled at ≤0.0020%.
[0025] Cu is also an austenite stabilizing element. Adding Cu can also reduce the Ar3 point temperature, improve the hardenability of the steel plate (hardenability of the composite reinforced steel plate), the atmospheric corrosion resistance and the low-temperature toughness of the steel plate; however, if the Cu addition is too much, higher than 0.45%, it is easy to cause copper brittleness, surface cracking of the ingot, internal cracking problems and especially deterioration of the SR performance of the welded joints of the ultra-high strength steel plate; for 1000MPa grade ultra-high strength quenched and tempered steel plates, if the Cu addition is too little, lower than 0.15%, any effect is very small; therefore, the Cu content is controlled between 0.15% and 0.45%. The composite addition of Cu and Ni can not only reduce the copper embrittlement of copper-containing steel and alleviate the intergranular cracking during the hot rolling process, but more importantly, Cu and Ni are both austenite stabilizing elements. The composite addition of Cu and Ni can significantly reduce Ar3 and increase the driving force for the phase transformation from austenite to ferrite, resulting in the growth of martensite / bainite laths in all directions, leading to a larger orientation difference between martensite / bainite blocks (i.e., increasing the V1 / V2 grain boundary ratio), and increasing the resistance of cracks passing through martensite / bainite laths.
[0026] Adding Ni can not only improve the mobility of dislocations in the ferrite phase and promote dislocation cross-slip, but also increase the orientation difference between the martensite / bainite block structures (i.e., increase the V1 / V2 grain boundary ratio); Ni, as an austenite stabilizing element, reduces the Ar3 point temperature, promotes the formation of lower bainite, disperses and refines the precipitation of carbides, and refines the size of the martensite / bainite packet structure. Therefore, Ni has the function of simultaneously improving the strength, elongation, low-temperature toughness and resistance to strain aging embrittlement of quenched and tempered steel plates; adding Ni to steel can also reduce the copper embrittlement phenomenon of copper-containing steel, alleviate intergranular cracking during hot rolling, and improve the atmospheric corrosion resistance of steel plates. Therefore, theoretically, the higher the Ni content in steel is within a certain range, the better. However, too high Ni content will harden the welding heat affected zone, which is not good for the weldability of the steel plate and the SR performance of the welded joint. However, for ultra-high strength 1000MPa grade quenched and tempered steel plates, there must be enough Ni content to ensure that the steel plate has sufficient hardenability and uniform performance in the thickness direction, while ensuring the plastic toughness and strain aging embrittlement resistance of the steel plate. Therefore, the Ni content is controlled between 1.50% and 2.20% to ensure the hardenability of the steel plate and the strength and toughness of the steel plate, as well as the strain aging embrittlement resistance without damaging the weldability of the steel plate.
[0027] Cr is a weak carbide-forming element. Although the addition of Cr improves the hardenability of the steel plate and promotes the formation of martensite / bainite, it reduces the orientation difference between martensite / bainite laths (i.e., increases the V1 / V4 grain boundary ratio) and reduces the resistance of cracks passing through the martensite / bainite packet structure. While improving the strength of the steel plate, it has a certain effect of deteriorating the toughness of the steel plate and the resistance to strain aging embrittlement. In addition, when the amount of Cr added is too much, the weldability of the steel plate, especially the SR performance of the welded joint, is seriously damaged. However, for ultra-high strength 1000MPa grade quenched and tempered steel plates, a certain Cr content must be present to ensure that the steel plate has sufficient hardenability and matches the strength and toughness of the steel plate. Therefore, the Cr content is controlled between 0.45% and 0.70%.
[0028] Adding Mo improves the hardenability and strength of the steel plate and promotes the formation of martensite / bainite. However, as a strong carbide-forming element, Mo increases the size of the martensite / bainite packet while promoting the formation of martensite / bainite, and the orientation difference between the formed martensite / bainite blocks is very small (i.e., increasing the V1 / V4 grain boundary ratio), reducing the resistance of cracks passing through the martensite / bainite packet structure. In addition, Mo promotes overquenching of the surface (sub) layer of ultra-high strength steel; therefore, while Mo greatly improves the strength of the steel plate, it reduces the low-temperature toughness, strain aging embrittlement resistance, and elongation of the ultra-high strength steel plate, inducing overquenching of the surface (sub) layer of the steel plate; and when Mo is added too much, it not only seriously damages the elongation, weldability and SR performance of the steel plate, but also increases the SR brittleness and production cost of the steel plate; however, for ultra-high strength 1000MPa grade ultra-high strength quenched and tempered steel plates, a certain Mo content must be present to ensure that the steel plate has sufficient hardenability and resistance to temper softening. Therefore, considering the phase transformation strengthening effect of Mo and its influence on the low-temperature toughness, elongation and weldability of the base steel plate, the Mo content is controlled between 0.35% and 0.60%.
[0029] The V content is between 0.030% and 0.060%, and as the thickness of the steel plate increases, the V content can be appropriately taken to the upper limit. The purpose of adding V is to improve the strength of the ultra-high strength quenched and tempered steel plate by dispersing and precipitating V (C, N) in the bainite / martensite laths. If V is added too little, less than 0.030%, too little V (C, N) is precipitated, and the strength of the ultra-high strength quenched and tempered steel plate cannot be effectively improved; if V is added too much, higher than 0.060%, the steel plate's low-temperature toughness, strain aging embrittlement resistance, elongation, weldability and welding SR performance will be damaged.
[0030] The purpose of adding a trace amount of Nb element in steel is to carry out non-recrystallization controlled rolling, refine the microstructure of the steel plate and increase the frequency of the phase transformation variant V1 / V2, improve the quenching structure of the surface (sub) layer of the steel plate, prevent excessive quenching of the surface (sub) layer of the steel plate, and improve the low-temperature toughness and strain aging embrittlement resistance of the steel plate. When the Nb addition is less than 0.010%, the controlled rolling effect cannot be effectively exerted; when the Nb addition exceeds 0.030%, the formation of upper bainite (Bu) and the secondary precipitation embrittlement of Nb (C, N) are induced under welding conditions, which seriously damages the low-temperature toughness of the heat affected zone (HAZ) of high heat input welding. Therefore, the Nb content is controlled between 0.010% and 0.030%, so as to obtain the best controlled rolling effect, realize the strength-toughness / strength-plasticity matching of ultra-high strength quenched and tempered steel plates, the strain aging embrittlement resistance and prevent excessive quenching of the surface (sub) layer, without damaging the toughness of the multi-layer and multi-pass welded HAZ.
[0031] Als in steel plates can fix the free [N] in steel, reduce the free [N] in the heat affected zone (HAZ) of welding, and improve the low-temperature impact toughness of multi-layer and multi-pass welded HAZ; however, adding excessive Als to steel will not only form a large number of dispersed needle-shaped Al2O3 inclusions in the steel, but also damage the low-temperature impact toughness and weldability of the steel plate. According to the analysis of the steel plate composition system, the optimal Als content is controlled between 0.030% and 0.060%.
[0032] In order to prevent excessive quenching of the steel plate surface, the formation of coarse martensite structure and ensure that the orientation difference between martensite / bainite blocks becomes larger (i.e., increase the V1 / V2 grain boundary ratio), the B content shall not exceed 0.0004%.
[0033] In order to ensure the surface quality of the invention steel plate slab and inhibit the occurrence of star cracks and edge cracks on the steel plate surface, the nitrogen content in the steel is ≤0.0040%.
[0034] In order to ensure the plastic toughness and resistance to strain aging embrittlement of ultra-high strength quenched and tempered steel plates, the inclusions in the steel must be reduced, among which alumina inclusions are the most harmful, so the O content in the steel is ≤0.0030%.
[0035] Ca treatment of steel can, on the one hand, further purify the molten steel, and on the other hand, modify the sulfides in the steel to make them non-deformable, stable and fine spherical sulfides, inhibit the hot brittleness of S, improve the low-temperature toughness, elongation and Z-direction properties of the steel plate, improve the anisotropy of the toughness and weldability of the steel plate. In addition, Ca treatment is used to improve the pouring of high-acid-soluble aluminum molten steel; the amount of Ca added depends on the S content in the steel. If the Ca addition is too low, the treatment effect is not great; if the Ca addition is too high, the size of the Ca(O,S) formed is too large, the brittleness is also increased, and it can become the starting point of the fracture crack, reducing the low-temperature toughness, strain aging embrittlement resistance, elongation and weldability of the steel plate, while also reducing the purity of the steel and polluting the molten steel. Generally, the Ca content is controlled according to ESSP = (wt%Ca) [1-1.24 (wt%O)] / 1.25 (wt%S), where ESSP is the sulfide inclusion shape control index, and the value range is preferably between 0.80 and 4.00. Therefore, the appropriate range of Ca content is 0.0010% to 0.0035%.
[0036] Therefore, the weight percentage of the composition elements of 1000MPa grade steel plates with high toughness, resistance to strain aging embrittlement and excellent weldability is: C: 0.07%~0.11%, Si: ≤0.15%, Mn: 0.85%~1.10%, P: ≤0.012%, S: ≤0.0020%, Cu: 0.15%~0.45%, Ni: 1.50%~2.20%, Cr: 0.45%~0.70%, Mo: 0.35%~0.60%, V: 0.030%~0.060%, Nb: 0.010%~0.030%, Als: 0.030%~0.060%, B: ≤0.0004%, N: ≤0.0040%, O: ≤0.0030%, Ca: 0.0010%~0.0035%, The rest are Fe and other unavoidable impurities; and the contents of the above elements satisfy the following relationship at the same time: [(%Mn)+0.69(%Ni)] / (%C)≥21.5; refine the fine structure of the microstructure and substructure of the ultra-high strength steel plate (i.e. refine the packet crystal size and increase the V1 / V2 ratio on the block boundary), improve the proportion, distribution and state of the second phase organization, improve the low-temperature plasticity and toughness, strong toughness / strong plasticity matching and resistance to strain aging embrittlement characteristics, while at the same time, the plasticity and toughness in the thickness direction of the steel plate (especially the center of the plate thickness) are uniform and excellent, and the ductile-brittle transition temperature of the fracture is lower than -60℃, ensuring that the steel plate has excellent crack resistance and crack arrest characteristics.
[0037] (%C)×[(6.53(%Si)+5.17(%Als)+1.55(%Mn)+10.67(%P)+26.39(%S)+25.3(%O)]≤0.205; A) Greatly reduce the damage of P, S, O inclusion elements to the plastic toughness and strain aging embrittlement resistance of steel plates; B) Reduce the degree of co-segregation of C, Mn, P, S and O during the solidification of molten steel, improve the low-temperature toughness, strain aging embrittlement resistance and weldability of the base steel plate; C) Inhibit the precipitation of MA islands in the HAZ during welding, reduce the size of MA islands in the HAZ, reduce the number of MA islands in the HAZ and improve their morphology and distribution, greatly Improve the low-temperature toughness and crack resistance and arrest properties of the welded HAZ; D) Inhibit excessive quenching of the surface (sub) layer of high-strength steel plates, improve the low-temperature toughness and environmental brittleness of the surface (sub) layer of steel plates, and improve the crack resistance and arrest properties of steel plates and the resistance to strain aging embrittlement; F) Balance the hardenability of the steel plate in the thickness direction, increase the critical cooling rate of the martensitic phase transformation, promote the lower bainite phase transformation, realize the "lower bainite---martensite" time continuity, effectively divide the original austenite grains, inhibit the generation of coarse martensitic crystal group packet size, increase the frequency of phase transformation variant pairs between V1 / V2, refine the block size, and improve the strength-toughness / strength-plasticity matching, elongation and low-temperature toughness of high-strength quenched and tempered steel plates.
[0038] Ca / S is between 1.00 and 3.00 and (%Ca)×(%S) 0.18 ≤1.5×10 -3 . Ensure sulfide spheroidization and minimize the influence of inclusions on low-temperature toughness, strain aging embrittlement resistance and weldability, while achieving high efficiency of inclusions: Ca (O, S) particles are evenly and finely distributed in the steel, inhibiting the growth of austenite grains in the heat-affected zone of slab heating and high heat input welding, ensuring uniform and fine microstructure of the steel plate, reducing the anisotropy of the longitudinal and transverse properties (strength, toughness) of the steel plate, improving the low-temperature toughness and strain aging embrittlement resistance of the steel plate, and improving the low-temperature toughness and crack resistance and crack arrest properties of the heat-affected zone of multi-layer and multi-pass welding of the steel plate.
[0039] Preferably, the steel plate has a tensile strength ≥950 MPa, a yield strength ≥890 MPa, a -60°C transverse impact energy ≥70 J, a -40°C aging transverse impact energy ≥70 J, and a fracture elongation δ5 ≥15%.
[0040] More preferably, the thickness of the steel plate is ≥20 mm.
[0041] As a preferred embodiment 2: a method for manufacturing a 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, for preparing the above-mentioned 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, comprising the following steps: Step 1: Smelting: According to the composition of claim 1, continuous casting is adopted, the tundish pouring superheat ΔT is controlled at 15°C to 30°C, the pulling speed is controlled at 0.5m / min to 1.0m / min, and the crystallizer liquid level fluctuation is controlled at ≤3mm; Step 2: Rolling: The first stage is ordinary rolling, the slab heating temperature is controlled at 1100℃~1170℃, the rolling reduction ratio is ≥4.0, and the rolling width ratio ζ is ≥1.4; to ensure that Nb in the steel is completely dissolved and the slab grains do not grow abnormally; to ensure that the microstructure of the rolling intermediate slab is uniform and fine, creating conditions for the second stage of controlled rolling to refine and homogenize the non-recrystallized grains; The second stage adopts controlled rolling, with the start rolling temperature of controlled rolling ≤830℃, the rolling pass reduction rate ≥8%, the cumulative reduction rate of the non-crystallized zone with a temperature of ≤830℃ ≥50%, and the final rolling temperature of 750℃~800℃; in order to accumulate sufficient deformation in the non-recrystallized austenite and form a high-density dislocation network structure, to form fine and uniform reversed austenite during heating during the quenching process of the steel plate, and then to evenly refine the microstructure of the final finished steel plate; Step 3: Cooling: After the controlled rolling is completed, the steel plate is slowly cooled. The slow cooling process is to keep the steel plate surface temperature ≥310℃ for more than 24 hours, and then the steel plate is naturally cooled to room temperature: Step 4: Quenching and tempering process: The off-line quenching and tempering process is adopted for production. The quenching temperature of the steel plate is dynamically adjusted according to the hardenability index of the steel plate and the Ac3 point temperature to achieve the matching between the hardenability of the steel plate, the quenching temperature and the quenching roller speed; the overquenching of the steel plate surface is suppressed to obtain a fine and uniform low-carbon martensite + a small amount of low-carbon lower bainite structure to obtain the performance requirements of the invented steel plate; Quenching: quenching temperature is 840~870℃, quenching time in the furnace is ≥2.0H minutes, H is the thickness of the finished steel plate, and the quenching roller speed is 2.0m / min~4.0m / min; Tempering: the tempering temperature of the steel plate is 575℃~615℃, the tempering time in the furnace is ≥ the quenching time in the furnace is ≥3.0H minutes, and H is the thickness of the finished steel plate; After tempering, the steel plate is naturally cooled to room temperature.
[0042] Preferably, step one also includes: to ensure that the as-cast structure of the slab is fully crushed, the microstructure of the ultra-high strength quenched and tempered steel plate is uniform and fine, and the anisotropy of the longitudinal and transverse properties is low, the surface layer of the steel plate has a certain strain storage rate, and the total compression ratio of the steel plate, that is, the slab thickness / finished steel plate thickness is ≥4.0, and the total width ratio is ≥1.4.
[0043] Preferably, the step 2 also satisfies the following relationship: ; in, is the cumulative reduction rate without recrystallization, unit: % ζ is the rolling width ratio, unit is %; T 终轧 is the final rolling temperature, in °C; H is the thickness of the finished steel plate in mm.
[0044] 1) With the increase of Nb content, the recrystallization stop temperature increases, the ability to inhibit the recovery recrystallization of the deformed austenite structure is enhanced, the dislocation density of the deformed austenite structure increases, the phase deformation nucleus increases, the degree of microstructure refinement after phase transformation increases, and the low-temperature toughness and crack resistance and crack arrest properties of the steel plate increase; 2) With the increase of the cumulative reduction rate of non-recrystallization ( , unit is %), the deformation degree of austenite structure is enhanced, the dislocation density of austenite structure is increased, the phase deformation nucleus points are increased, the microstructure refinement degree after phase transformation is increased, and the low-temperature toughness and crack resistance and crack arrest properties of the steel plate are increased; 3) With the increase of rolling width ratio (ζ, unit is %), the crushing ability of the cast structure is enhanced, the grain refinement degree of the steel plate is increased, (100) <011> The texture is greatly weakened, the longitudinal and transverse anisotropy of the steel plate is sharply reduced, the low-temperature toughness and strain aging embrittlement resistance of the steel plate are improved, and the uniformity of the longitudinal and transverse performance is improved; 4) With the increase of [(%Mn)+0.69(%Ni) / (%C), the microstructure refinement ability is enhanced, the phase transition point Ar3 temperature is reduced, the microstructure after phase transformation is refined, the size of the precipitated carbides is reduced, and the strength and low-temperature toughness of the quenched and tempered steel plate are improved; 5) With the increase of the final rolling temperature (T 终轧, in ℃) increases, the recovery and recrystallization speed of the deformed austenite structure increases, the dislocation density in the austenite structure decreases sharply, the phase deformation nuclei also decreases sharply, the coarsening degree of the microstructure increases after the phase transformation, and the low-temperature toughness and crack resistance and crack arrest characteristics of the steel plate deteriorate; 6) As the thickness of the finished steel plate (H, in mm) increases, the degree of rolling deformation penetration decreases, the dislocation density of the deformed structure decreases, the phase deformation nuclei also decreases sharply, the coarsening degree of the microstructure increases after the phase transformation, and the low-temperature toughness and crack resistance and crack arrest characteristics of the steel plate deteriorate. In summary, when the above formula is met, the low-temperature toughness, strain aging embrittlement resistance and low longitudinal and transverse anisotropy of the steel plate can be ensured.
[0045] Preferably, the step 4 also satisfies the following relationship: 0.31≤{[(T 淬火 )-(Ac3)]×DI} / [(V 淬火 )×ln(t 淬火 )×PT]}≤0.43; Among them, T 淬火 is the quenching and holding temperature, in °C; Ac3 is the temperature at which the austenite transformation is completed, in °C; DI is the hardenability index, in mm; V 淬火 is the roller speed of quenching, in m / min; t 淬火 is the quenching time in the furnace, in min; PT is the tempering characteristic parameter.
[0046] As a more preferred embodiment, the austenite transformation completion temperature Ac3 in step 4 also satisfies the following relationship: Ac3=910-203(%C) 0.5 +44.7(%Si)-15.2(%Ni)+31.5(%Mo)+104(%V)+13.1(%W)-[30(%Mn)+11(%Cr)+20(%Cu)-700(%P)-400(%Al)-120(%As)-400(%Ti)].
[0047] Furthermore, the hardenability index DI in step 4 also satisfies the following relationship: DI=0.367C 0.5 [(1+0.7(%Si)][(1+3.33(%Mn)][(1+0.35(%Cu)][(1+0.36(%Ni)][(1+2.1 6(%Cr)][(1+3(%Mo)][(1+1.75(%V)][(1+1.77(%Al)][(1+200(%B)]×25.4.
[0048] Furthermore, the tempering characteristic parameter PT in step 4 also satisfies the following relationship: PT=(T 回火 )[20+lg(t 回火 )]; Among them, T 回火 is the tempering temperature, in K; t 回火 Tempering time in the furnace, in min 1) The matching between quenching temperature, hardenability index, quenching time and quenching speed is achieved, which reduces the problem of excessive quenching of the surface (sub-surface) of ultra-high strength quenched and tempered steel plates, inhibits the martensitic phase transformation, especially the appearance of coarse martensitic structure, and promotes the lower bainite phase transformation; it not only fully refines the martensitic crystal cluster size packet, but also increases the proportion of large-angle grain boundaries between blocks, promotes the formation of martensite + lower bainite complex phase structure, and ensures that the steel plate has excellent low-temperature toughness, crack arrest characteristics and resistance to strain aging embrittlement degradation; 2 ) balances the hardenability of ultra-high strength steel plates of different thicknesses, ensuring that the ultra-high strength quenched and tempered steel plates have sufficient hardenability and strength, while achieving uniform microstructure, high toughness and strong toughness / strong plasticity matching in the thickness direction of the quenched and tempered steel plates; 3) by matching and regulating the tempering parameter PT with the quenching temperature, hardenability index, quenching time and quenching speed, excessive quenching of the steel plate surface (sub-surface) is suppressed. The quenched and tempered steel plates exceeding the strength not only have excellent low-temperature toughness and resistance to strain aging embrittlement, but also improve the steel plate's strong toughness / strong plasticity matching.
[0049] As a preferred embodiment 3, the steel sample is the newly invented steel 1, the plate thickness is 20 mm, and its composition is shown in Table 1; As a preferred embodiment 4, the steel sample is the newly invented steel 2, the plate thickness is 40 mm, and its composition is shown in Table 1; As a preferred embodiment 5, the steel sample is the newly invented steel 3, the plate thickness is 60 mm, and its composition is shown in Table 1; As a preferred embodiment 6, the steel sample is the newly invented steel 4, the plate thickness is 80 mm, and its composition is shown in Table 1; Figure 1 As shown in the figure, from the fine structure of the full thickness microstructure of the steel plate, it can be seen that the microstructure of the finished steel plate is fine low-carbon tempered martensite + a small amount of tempered lower bainite, and the average crystal group packet size is below 20μm; it not only achieves the matching of ultra-high strength and toughness / plasticity, resistance to strain aging embrittlement, and weldability, but also solves the problem of excessive quenching of the surface (sub) layer of ultra-high strength steel plates. The steel plate is particularly suitable for large steel structures and equipment such as penstocks, steel bifurcated pipes, volutes, marine structures and large engineering machinery in hydropower projects; As a preferred embodiment 7, the steel sample is the newly invented steel 5, the plate thickness is 100 mm, and its composition is as follows: Figure 2 As shown in Table 1;
[0050] Table 1 The smelting and rolling one-stage process of Example 3 to Example 7 is as follows Figure 3 As shown in Table 2;
[0051] Table 2 The rolling two-stage process of Example 3 to Example 7 is as follows Figure 4 As shown in Table 3;
[0052] Table 3 The quenching and tempering process of Example 3 to Example 7 is as follows Figure 5 As shown in Table 4;
[0053] Table 4 The steel plate performance tests of Examples 3 to 7 are as follows: Figure 6 As shown in Table 5;
[0054] Table 5.
Claims
1. 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability, characterized by: The weight percentages of the constituent elements are: C:0.07%~0.11%, Si: ≤0.15%, Mn: 0.85%~1.10%, P:≤0.012%, S:≤0.0020%, Cu: 0.15%~0.45%, Ni: 1.50%~2.20%, Cr:0.45%~0.70%, Mo: 0.35%~0.60%, V:0.030%~0.060%, Nb: 0.010%~0.030%, Als: 0.030%~0.060%, B:≤0.0004%, N:≤0.0040%, O:≤0.0030%, Ca: 0.0010%~0.0035%, The rest are Fe and other unavoidable impurities; and the contents of the above elements satisfy the following relationship at the same time: [(%Mn)+0.69(%Ni)] / (%C)≥21.5; (%C)×[(6.53(%Si)+5.17(%Als)+1.55(%Mn)+10.67(%P)+26.39(%S)+25.3(%O)]≤0.205; Ca / S is between 1.00 and 3.00 and (%Ca)×(%S) 0.18 ≤1.5×10 -3 .
2. The 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 1, characterized in that: The steel plate has a tensile strength of ≥950MPa, a yield strength of ≥890MPa, a -60°C transverse impact energy of ≥70J, a -40°C aging transverse impact energy of ≥70J, and a fracture elongation δ5 of ≥15%.
3. The 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 2, characterized in that: The thickness of the steel plate is ≥20 mm.
4. A method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability, characterized in that: The method for preparing the 1000MPa grade steel plate with high toughness, resistance to strain aging embrittlement and excellent weldability as claimed in any one of claims 1 to 3 comprises the following steps: Step 1: Smelting: According to the composition of claim 1, continuous casting is adopted, the tundish pouring superheat ΔT is controlled at 15°C to 30°C, the pulling speed is controlled at 0.5m / min to 1.0m / min, and the crystallizer liquid level fluctuation is controlled at ≤3mm; Step 2: Rolling: The first stage is ordinary rolling, the slab heating temperature is controlled at 1100℃~1170℃, the rolling reduction ratio is ≥4.0, and the rolling width ratio ζ is ≥1.4; The second stage adopts controlled rolling, with the start rolling temperature of controlled rolling ≤830℃, the rolling pass reduction rate ≥8%, the cumulative reduction rate of the non-crystallized zone with a temperature of ≤830℃ ≥50%, and the final rolling temperature of 750℃~800℃; Step 3: Cooling: After the controlled rolling is completed, the steel plate is slowly cooled. The slow cooling process is to keep the steel plate surface temperature ≥310℃ for more than 24 hours, and then the steel plate is naturally cooled to room temperature: Step 4: Quenching and tempering process: The off-line quenching and tempering process is used for production. The quenching temperature of the steel plate is dynamically adjusted according to the hardenability index of the steel plate and the Ac3 point temperature to achieve a match between the hardenability of the steel plate, the quenching temperature and the quenching roller speed; Quenching: quenching temperature is 840~870℃, quenching time in the furnace is ≥2.0H minutes, H is the thickness of the finished steel plate, and the quenching roller speed is 2.0m / min~4.0m / min; Tempering: the tempering temperature of the steel plate is 575℃~615℃, the tempering time in the furnace is ≥ the quenching time in the furnace is ≥3.0H minutes, and H is the thickness of the finished steel plate; After tempering, the steel plate is naturally cooled to room temperature.
5. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 4, characterized in that: The step one also includes: to ensure that the as-cast structure of the slab is fully crushed, the microstructure of the ultra-high strength quenched and tempered steel plate is uniform and fine, the anisotropy of the longitudinal and transverse properties is low, the surface layer of the steel plate has a certain strain storage rate, and the total compression ratio of the steel plate, that is, the slab thickness / finished steel plate thickness is ≥4.0, and the total width ratio is ≥1.
4.
6. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 4, characterized in that: The step 2 also satisfies the following relationship: ; in, is the cumulative reduction rate without recrystallization, unit: % ζ is the rolling width ratio, unit is %; T 终轧 is the final rolling temperature, in °C; H is the thickness of the finished steel plate in mm.
7. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 4, characterized in that: The step 4 also satisfies the following relationship: 0.31≤{[(T 淬火 )-(Ac3)]×DI} / [(V 淬火 )×ln(t 淬火 )×PT]}≤0.43; Among them, T 淬火 is the quenching and holding temperature, in °C; Ac3 is the temperature at which the austenite transformation is completed, in °C; DI is the hardenability index, in mm; V 淬火 is the roller speed of quenching, in m / min; t 淬火 is the quenching time in the furnace, in min; PT is the tempering characteristic parameter.
8. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 7, characterized in that: The austenite transformation completion temperature Ac3 in step 4 also satisfies the following relationship: Ac3=910-203(%C) 0.5 +44.7(%Si)-15.2(%Ni)+31.5(%Mo)+104(%V)+13.1(%W)-[30(%Mn)+11(%Cr)+20(%Cu)-700(%P)-400(%Al)-120(%As)-40(%Ti)] 9. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 8, characterized in that: The hardenability index DI in step 4 also satisfies the following relationship: DI=0.367C 0.5 [(1+0.7(%Si)][(1+3.33(%Mn)][(1+0.35(%Cu)][(1+0.36(%Ni)][(1+2.16(%Cr)][(1+3(%Mo)][(1+1.75(%V)][(1+1.77(%Al)][(1+200(%B))]×25.4).
10. The method for manufacturing a 1000MPa grade steel plate having high toughness, resistance to strain aging embrittlement and excellent weldability according to claim 9, characterized in that: The tempering characteristic parameter PT in step 4 also satisfies the following relationship: PT=(T 回火 )[20+lg(t 回火 )]; Among them, T 回火 is the tempering temperature, in K; t 回火 Tempering time in the furnace, in minutes.
Citation Information
Patent Citations
Low-cost ultra-thick 1000MPa-grade steel plate and manufacturing method thereof
CN113832387A
1000MPa-grade steel plate with matched obdurability / strength plasticity and manufacturing method of 1000MPa-grade steel plate
CN118086779A
HT550 steel plate with ultrahigh toughness and excellent weldability and manufacturing method of the same
US20160122844A1