GH3536 high-temperature alloy material and heat treatment method thereof

Through the combination of thermal isostatic pressure, homogenization and solid solution treatment, the problem of poor toughness of the laser selection melt forming GH3536 high-temperature alloy material is solved, and the excellent mechanical properties and high-temperature long-lasting time are achieved at room temperature and high temperature are achieved, improving the The comprehensive performance of the material.

CN119082633APending Publication Date: 2024-12-06AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411206666.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing heat treatment process cannot meet the comprehensive mechanical properties requirements of the GH3536 high-temperature alloy material in the laser selection melt forming, resulting in poor toughness and inability to meet the usage requirements.

Method used

The combination of thermal isostatic pressure treatment, homogenization treatment and solid solution treatment is adopted. The specific steps include applying a pressure of 150 to 170MPa at 1150 to 1250°C for thermal isostatic pressure treatment, and then homogenization treatment is performed at 1200 to 1300°C. , and the solution treatment was carried out at 1100-1160°C, and finally cooled to room temperature.

Benefits of technology

Through this method, GH3536 high-temperature alloy material exhibits excellent comprehensive mechanical properties under room temperature and high temperature conditions, including improving toughness and meeting the requirements of high-temperature durability ≥24h, eliminating microcrack defects in forming forms, disappearing the molten pool structure, and branches The crystal dissolves and carbides precipitate, improving the mechanical properties as a whole.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082633A_ABST
    Figure CN119082633A_ABST
Patent Text Reader

Abstract

The invention discloses a GH3536 high-temperature alloy material and a heat treatment method thereof, and belongs to the technical field of heat treatment of high-temperature alloy elements. The method solves the problem that the GH3536 high-temperature alloy material subjected to SLM forming is poor in toughness and cannot meet the use requirement by adopting an existing heat treatment process to treat the GH3536 high-temperature alloy material subjected to SLM forming. The heat treatment method of the GH3536 high-temperature alloy material, provided by the invention, comprises the following steps: step 1, carrying out hot isostatic pressing treatment on the GH3536 high-temperature alloy material, and then cooling along with a furnace; 2, the GH3536 high-temperature alloy material is subjected to homogenization treatment after hot isostatic pressing treatment, and then furnace cooling is carried out; and 3, after homogenization treatment, the GH3536 high-temperature alloy material is subjected to solution treatment, then furnace cooling is conducted, and finally the GH3536 high-temperature alloy material subjected to heat treatment is obtained. According to the heat treatment method provided by the invention, the comprehensive mechanical property of the GH3536 high-temperature alloy material for additive manufacturing can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat treatment of high temperature alloys, and in particular to a GH3536 high temperature alloy material and a heat treatment method thereof. Background Art

[0002] GH3536 high-temperature alloy material is a nickel-based high-temperature alloy material with high iron content strengthened by chromium and molybdenum solid solution, which has good oxidation resistance and corrosion resistance. The existing traditional manufacturing technology cannot meet the requirements of complex structure of high-temperature alloy components. Selective laser melting (SLM) is the main technical approach for additive manufacturing of metal materials and can be used to manufacture high-temperature alloy components with complex shapes.

[0003] At present, the GH3536 high-temperature alloy material formed by SLM still uses a heat treatment process that is compatible with the traditional manufacturing process. Since the raw materials of the SLM forming process and the traditional manufacturing process are completely different, the microstructure characteristics and mechanical properties of the SLM-formed high-temperature alloy material are greatly different from those of the traditional manufacturing process. Therefore, using the heat treatment process of the traditional manufacturing process for the SLM-formed GH3536 high-temperature alloy material will result in a decrease in the performance of the SLM-formed GH3536 high-temperature alloy material and cannot meet the use requirements.

[0004] Therefore, it has good application prospects to study and develop a heat treatment method that matches SLM forming technology and can improve the comprehensive mechanical properties of GH3536 high-temperature alloy materials. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a heat treatment method for GH3536 high-temperature alloy material, so as to solve the technical problem that the existing heat treatment process for SLM-formed GH3536 high-temperature alloy material leads to poor toughness and cannot meet the use requirements.

[0006] The purpose of the present invention is mainly achieved through the following technical solutions:

[0007] The present invention provides a heat treatment method for a GH3536 high temperature alloy material, comprising the following steps:

[0008] Step 1, subjecting the GH3536 high temperature alloy material to hot isostatic pressing treatment, and then cooling it in the furnace;

[0009] Step 2, homogenizing the GH3536 high temperature alloy material, and then cooling it in the furnace;

[0010] Step 3: subjecting the GH3536 high temperature alloy material to solid solution treatment, and then cooling it in the furnace to finally obtain the heat-treated GH3536 high temperature alloy material.

[0011] Furthermore, in step 1, the GH3536 high-temperature alloy material is a GH3536 high-temperature alloy material formed by laser selective melting.

[0012] Furthermore, in step 1, the components and mass percentages of the GH3536 high temperature alloy material formed by laser selective melting are: Cr 19.5%-21.2%, Mo 8.02%-10.4%, Fe

[0013] 17.79%-19.4%, Co 1.32%-1.54%, C 0.11%-0.13%, W 0.55%-0.71%, Mn 0.02%-0.03%, Si 0.3%-0.35%, and the rest is Ni.

[0014] Furthermore, in step 1, during the hot isostatic pressing treatment, the GH3536 high-temperature alloy material is first placed in a closed hot isostatic pressing device, and an isotropic pressure of 150 to 170 MPa is applied to the GH3536 high-temperature alloy material.

[0015] Furthermore, in step 1, the temperature of the GH3536 high temperature alloy material during hot isostatic pressing is 1150-1250°C.

[0016] Furthermore, in step 1, the hot isostatic pressing treatment of the GH3536 high temperature alloy material is performed for a treatment time of 2 to 4 hours.

[0017] Furthermore, in step 1, the pressure of the GH3536 high temperature alloy material during hot isostatic pressing is 155-165 MPa.

[0018] Furthermore, in step 1, the temperature of the GH3536 high temperature alloy material during hot isostatic pressing is 1180-1220°C.

[0019] Furthermore, in step 1, the GH3536 high temperature alloy material is subjected to hot isostatic pressing for 2.5 to 3.5 hours.

[0020] On the other hand, the present invention further provides a GH3536 high-temperature alloy material, which is obtained by heat treatment using the above-mentioned heat treatment method for the GH3536 high-temperature alloy material.

[0021] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0022] (1) The heat-treated GH3536 high-temperature alloy material obtained by the present invention has excellent comprehensive mechanical properties at room temperature and high temperature conditions, and can meet the requirement of high-temperature endurance time ≥ 24h.

[0023] (2) Hot isostatic pressing treatment is first performed to heal the microcrack defects in the as-formed GH3536 alloy. Then, homogenization treatment is performed to make the molten pool structure in the GH3536 alloy disappear, the dendrites are completely dissolved, and the small columnar crystals grow together to become equiaxed crystals. The XY plane grain distribution in the GH3536 alloy shows the phenomenon of alternating arrangement of coarse equiaxed crystal areas and fine equiaxed crystal areas, eliminating the anisotropy of the as-formed GH3536 alloy. Finally, solution treatment is performed to precipitate irregular blocky carbides at the grain boundaries, and large-sized spherical carbides are scattered inside the grains. EDS analysis of the carbides shows that the carbides are M23C6 type carbides, which help to improve the overall mechanical properties of the GH3536 alloy sample, especially the toughness of the GH3536 alloy sample.

[0024] (3) The heat treatment method of the GH3536 high-temperature alloy material provided by the present invention has a simple process, low energy consumption, and is suitable for industrial applications.

[0025] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the embodiments of the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings are only for the purpose of illustrating specific embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0027] Figure 1 This is the microstructure diagram of the heat-treated GH3536 high-temperature alloy material obtained in Example 1;

[0028] Figure 2 This is the microstructure diagram of GH3536 alloy after hot isostatic pressing treatment. DETAILED DESCRIPTION

[0029] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0030] The present invention provides a heat treatment method for a GH3536 high temperature alloy material, comprising the following steps:

[0031] Step 1, subjecting the GH3536 high temperature alloy material to hot isostatic pressing, and then cooling it to room temperature with the furnace;

[0032] The above-mentioned GH3536 high-temperature alloy material is a GH3536 high-temperature alloy material formed by selective laser melting (SLM).

[0033] The components and mass percentages of the GH3536 high-temperature alloy material formed by laser selective melting are: Cr19.5%-21.2%, Mo 8.02%-10.4%, Fe 17.79%-19.4%, Co

[0034] 1.32%-1.54%, C 0.11%-0.13%, W 0.55%-0.71%, Mn 0.02%-0.03%, Si0.3%-0.35%, and the rest is Ni.

[0035] Furthermore, the components and mass percentages of the GH3536 high-temperature alloy material formed by the above-mentioned laser selective melting are: Cr 20.5%, Mo 9.02%, Fe 18.79%, Co 1.52%, C 0.12%, W 0.6%, Mn 0.02%, Si0.3%, and the rest is Ni; the forming equipment model is SLM-100, used in a nitrogen protection environment, the laser power is 200W, the scanning speed is 1000mm / s, the layer thickness is 30μm, the scanning spacing is 60μm, the scanning strategy is zigzag line-by-line scanning, and the deflection angle between adjacent layers is 67°.

[0036] In the above step 1, the temperature of the hot isostatic pressing treatment of the GH3536 high temperature alloy material is 1150-1250° C., the pressure of the hot isostatic pressing treatment is 150-170 MPa, and the time of the hot isostatic pressing treatment is 2-4 hours.

[0037] In the above step 1, when hot isostatic pressing is performed, the GH3536 high temperature alloy material is first placed in a closed hot isostatic pressing device, and an equal pressure of 150-170 MPa is applied to the GH3536 high temperature alloy material in all directions, and a high temperature of 1150-1250°C is applied at the same time, so that the GH3536 high temperature alloy material is sintered and densified. After the hot isostatic pressing treatment, the microcrack defects in the shaped GH3536 high temperature alloy are healed, such as Figure 2 As shown in the figure, no defects such as microcracks, pores and lack of fusion were observed in the GH3536 alloy after hot isostatic pressing.

[0038] In the above step 1, the hot isostatic pressing temperature is 1180-1220°C, for example, 1190°C, 1200°C, 1210°C; the hot isostatic pressing pressure is 155-165MPa, for example, 158MPa, 160MPa, 163MPa; the hot isostatic pressing time is 2.5-3.5h, for example, 2.8h, 3h, 3.3h; by limiting the hot isostatic pressing temperature, time and pressure, the present invention can obtain a GH3536 high-temperature alloy material with excellent comprehensive mechanical properties and high-temperature endurance performance.

[0039] Step 2: After the hot isostatic pressing treatment, the GH3536 high temperature alloy material is homogenized and then cooled to room temperature in the furnace;

[0040] In the above step 2, the temperature of the above homogenization treatment is 1200-1300°C, and the homogenization treatment time is 0.5-1.5h. Through the homogenization heat treatment, the molten pool structure in the GH3536 high temperature alloy material can be eliminated, the dendrites are completely dissolved, the fine columnar crystals merge and grow into equiaxed crystals, and the XY plane grain distribution of the GH3536 alloy shows the phenomenon of alternating arrangement of coarse equiaxed crystal areas and fine equiaxed crystal areas.

[0041] In the above step 2, the homogenization temperature is 1240-1260° C., for example, 1250° C. The homogenization time is 0.8-1.2 h, for example, 1 h. The increase of the homogenization temperature and the extension of the holding time increase the grain size of the GH3536 alloy.

[0042] In the above step 2, when the homogenization temperature is lower than 1200°C, for example, when the homogenization temperature is 1130 and 1160°C, the grains of the GH3536 alloy are relatively small, with a size of 40-70 μm; but when the homogenization temperature is 1200-1300°C, the grain size of the GH3536 sample grains is concentrated in the range of 90-100 μm, and the grain size of the GH3536 alloy becomes larger, which can meet the requirements.

[0043] Step 3: After the homogenization treatment, the GH3536 high temperature alloy material is subjected to a solid solution treatment, and then cooled to room temperature with the furnace to finally obtain the heat-treated GH3536 high temperature alloy material.

[0044] In the above step 3, the temperature of the solution treatment is 1100-1160° C., and the time of the solution treatment is 25-35 min.

[0045] In the above step 3, the solution treatment temperature is 1120-1140° C., for example, 1125° C., 1130° C., 1135° C.; and the solution treatment time is 28-32 min, for example, 30 min.

[0046] The present invention performs heat treatment on the GH3536 high-temperature alloy material formed by laser selective melting (SLM) in strict accordance with the sequence of isostatic pressing treatment, homogenization treatment and solution treatment, and the obtained GH3536 high-temperature alloy material has the best toughness; this is because: firstly hot isostatic pressing treatment can heal the microcrack defects in the morphological GH3536 alloy; then homogenization treatment is performed, the molten pool structure in the GH3536 alloy disappears, the dendrites are completely dissolved, the fine columnar crystals merge and grow into equiaxed crystals, and the XY plane grain distribution in the GH3536 alloy shows the phenomenon of alternating arrangement of coarse equiaxed crystal areas and fine equiaxed crystal areas, eliminating the anisotropy of the morphological GH3536 alloy; finally solution treatment is performed, irregular block carbides are precipitated at the grain boundaries, and larger-sized spherical carbides are scattered inside the grains. By performing EDS analysis on the carbides, it is confirmed that the carbides are M23C6 type carbides, and the M23C6 type carbides help to improve the toughness of the GH3536 alloy sample as a whole.

[0047] On the other hand, the present invention also provides a GH3536 high-temperature alloy material, which is obtained by heat treatment using the above-mentioned heat treatment method.

[0048] Example 1

[0049] This embodiment provides a heat treatment process for a GH3536 high temperature alloy material, using the above-mentioned heat treatment method for the GH3536 high temperature alloy material. The heat treatment process specifically includes:

[0050] Step 1, hot isostatic pressing the GH3536 high temperature alloy material, and then cooling it to room temperature with the furnace; the temperature of the hot isostatic pressing treatment is 1150° C., the pressure of the hot isostatic pressing treatment is 150 MPa, and the time of the hot isostatic pressing treatment is 2 hours;

[0051] The components and mass percentages of the GH3536 high-temperature alloy material formed by the above-mentioned laser selective melting are: Cr20.5%, Mo 9.02%, Fe 18.79%, Co 1.52%, C 0.12%, W 0.6%, Mn 0.02%, Si 0.3%, and the rest is Ni; the forming equipment model is SLM-100, used in a nitrogen protection environment, with a laser power of 200W, a scanning speed of 1000mm / s, a layer thickness of 30μm, a scanning spacing of 60μm, a zigzag line-by-line scanning strategy, and a deflection angle of 67° between adjacent layers.

[0052] Step 2: After the hot isostatic pressing treatment, the GH3536 high temperature alloy material is homogenized and then cooled to room temperature with the furnace; the homogenization temperature is 1200° C. and the homogenization time is 0.5 h;

[0053] Step 3: After homogenization treatment, the GH3536 high-temperature alloy material is subjected to solid solution treatment, and then cooled to room temperature with the furnace. The solid solution treatment temperature is 1100° C. and the solid solution treatment time is 25 min. Finally, the heat-treated GH3536 high-temperature alloy material is obtained.

[0054] The microstructure of the heat-treated GH3536 high-temperature alloy material obtained in this embodiment is shown in FIG. Figure 1 As shown by Figure 1 It can be seen that the precipitates at the grain boundaries of the heat-treated GH3536 high-temperature alloy material have become continuous chains, and a large number of small carbides are dispersed in the crystals; through energy scattering spectrum analysis of the carbides, it can be seen that the carbides have high contents of Cr and Mo, and are M23C6 type carbides and M6C type carbides.

[0055] Example 2

[0056] This embodiment provides a heat treatment process for a GH3536 high temperature alloy material, using the above-mentioned heat treatment method for the GH3536 high temperature alloy material. The heat treatment process specifically includes:

[0057] Step 1, hot isostatic pressing the GH3536 high temperature alloy material, and then cooling it to room temperature with the furnace; the hot isostatic pressing temperature is 1190° C., the hot isostatic pressing pressure is 155 MPa, and the hot isostatic pressing time is 2.5 h;

[0058] The components and mass percentages of the GH3536 high-temperature alloy material formed by the above-mentioned laser selective melting are: Cr20.5%, Mo 9.02%, Fe 18.79%, Co 1.52%, C 0.12%, W 0.6%, Mn 0.02%, Si 0.3%, and the rest is Ni; the forming equipment model is SLM-100, used in a nitrogen protection environment, with a laser power of 200W, a scanning speed of 1000mm / s, a layer thickness of 30μm, a scanning spacing of 60μm, a zigzag line-by-line scanning strategy, and a deflection angle of 67° between adjacent layers.

[0059] Step 2: After the hot isostatic pressing treatment, the GH3536 high temperature alloy material is homogenized and then cooled to room temperature with the furnace; the homogenization temperature is 1240° C. and the homogenization time is 0.8 h;

[0060] Step 3: After homogenization treatment, the GH3536 high-temperature alloy material is subjected to solid solution treatment, and then cooled to room temperature with the furnace. The solid solution treatment temperature is 1120° C. and the solid solution treatment time is 30 minutes; finally, the heat-treated GH3536 high-temperature alloy material is obtained.

[0061] Example 3

[0062] This embodiment provides a heat treatment process for a GH3536 high temperature alloy material, using the above-mentioned heat treatment method for the GH3536 high temperature alloy material. The heat treatment process specifically includes:

[0063] Step 1, hot isostatic pressing the GH3536 high temperature alloy material, and then cooling it to room temperature with the furnace; the hot isostatic pressing temperature is 1220° C., the hot isostatic pressing pressure is 165 MPa, and the hot isostatic pressing time is 3 hours;

[0064] The components and mass percentages of the GH3536 high-temperature alloy material formed by the above-mentioned laser selective melting are: Cr20.5%, Mo 9.02%, Fe 18.79%, Co 1.52%, C 0.12%, W 0.6%, Mn 0.02%, Si 0.3%, and the rest is Ni; the forming equipment model is SLM-100, used in a nitrogen protection environment, with a laser power of 200W, a scanning speed of 1000mm / s, a layer thickness of 30μm, a scanning spacing of 60μm, a zigzag line-by-line scanning strategy, and a deflection angle of 67° between adjacent layers.

[0065] Step 2: After the hot isostatic pressing treatment, the GH3536 high temperature alloy material is homogenized and then cooled to room temperature with the furnace; the homogenization temperature is 1280° C. and the homogenization time is 1.2 h.

[0066] Step 3: After homogenization treatment, the GH3536 high-temperature alloy material is subjected to solid solution treatment, and then cooled to room temperature with the furnace. The solid solution treatment temperature is 1140° C., and the solid solution treatment time is 32 minutes; finally, the heat-treated GH3536 high-temperature alloy material is obtained.

[0067] Example 4

[0068] This embodiment provides a heat treatment process for a GH3536 high temperature alloy material, using the above-mentioned heat treatment method for the GH3536 high temperature alloy material. The heat treatment process specifically includes:

[0069] Step 1, hot isostatic pressing the GH3536 high temperature alloy material, and then cooling it to room temperature with the furnace; the temperature of the hot isostatic pressing is 1250° C., the pressure of the hot isostatic pressing is 170 MPa, and the time of the hot isostatic pressing is 4 hours;

[0070] The components and mass percentages of the GH3536 high-temperature alloy material formed by the above-mentioned laser selective melting are: Cr20.5%, Mo 9.02%, Fe 18.79%, Co 1.52%, C 0.12%, W 0.6%, Mn 0.02%, Si 0.3%, and the rest is Ni; the forming equipment model is SLM-100, used in a nitrogen protection environment, with a laser power of 200W, a scanning speed of 1000mm / s, a layer thickness of 30μm, a scanning spacing of 60μm, a zigzag line-by-line scanning strategy, and a deflection angle of 67° between adjacent layers.

[0071] Step 2: After the hot isostatic pressing treatment, the GH3536 high-temperature alloy material is homogenized and then cooled to room temperature with the furnace; the homogenization temperature is 1300° C. and the homogenization time is 1.5 h.

[0072] Step 3: After homogenization treatment, the GH3536 high-temperature alloy material is subjected to solid solution treatment, and then cooled to room temperature with the furnace. The solid solution treatment temperature is 1160° C. and the solid solution treatment time is 35 minutes; finally, the heat-treated GH3536 high-temperature alloy material is obtained.

[0073] Comparative Example 1

[0074] The temperature of the hot isostatic pressing treatment in Example 1 is 1500° C., the time of the hot isostatic pressing treatment is 0.5 h, the temperature of the solution treatment is 1500° C., and other conditions remain unchanged.

[0075] Comparative Example 2

[0076] The hot isostatic pressing process in Example 1 was omitted, and the homogenization process was directly performed, while other conditions remained unchanged.

[0077] Comparative Example 3

[0078] The homogenization process in Example 1 is omitted, and the solid solution treatment is directly performed after the hot isostatic pressing treatment, and other conditions remain unchanged.

[0079] Comparative Example 4

[0080] The solution treatment process of Example 1 was omitted, and other conditions remained unchanged.

[0081] The tensile properties of the heat-treated GH3536 high-temperature alloy materials obtained in Examples 1 to 4 and Comparative Examples 1 to 4 and the SLM-formed GH3536 high-temperature alloy materials before heat treatment were tested at room temperature and high temperatures (650°C, 750°C and 815°C). The results are shown in Tables 1 to 4.

[0082] Table 1 Room temperature tensile properties test results of GH3536 high temperature alloy before and after heat treatment

[0083]

[0084] It can be seen from Table 1 that at room temperature, the transverse elongation after fracture of the heat-treated GH3536 high-temperature alloy material is 31.8%-37.9%, and the longitudinal elongation after fracture is 35.3%-38.6%. Compared with the untreated GH3536 high-temperature alloy material, the transverse and longitudinal elongations after fracture of the heat-treated GH3536 high-temperature alloy material at room temperature are greatly improved, which indicates that the toughness of the heat-treated GH3536 high-temperature alloy material is greatly improved.

[0085] Table 2 Tensile properties test results of GH3536 high temperature alloy material at 650℃ before and after heat treatment

[0086]

[0087] It can be seen from Table 2 that at 650°C, the transverse elongation after fracture of the heat-treated GH3536 high-temperature alloy material is 49.0%-358.5%, and the longitudinal elongation after fracture is 49.0-66.0%. Compared with the untreated GH3536 high-temperature alloy material, the transverse and longitudinal elongations after fracture of the heat-treated GH3536 high-temperature alloy material at 650°C are greatly improved, which indicates that the toughness of the heat-treated GH3536 high-temperature alloy material is greatly improved.

[0088] Table 3 Tensile properties test results of GH3536 superalloy material at 750℃ before and after heat treatment

[0089]

[0090]

[0091] It can be seen from Table 3 that at 750°C, the transverse elongation after fracture of the heat-treated GH3536 high-temperature alloy material is 45.5%-52.5%, and the longitudinal elongation after fracture is 45.0-55.5%. Compared with the untreated GH3536 high-temperature alloy material, the transverse and longitudinal elongations of the heat-treated GH3536 high-temperature alloy material at 750°C are greatly improved, which indicates that the toughness of the heat-treated GH3536 high-temperature alloy material is greatly improved.

[0092] Table 4 Tensile properties test results of GH3536 superalloy material at 815℃ before and after heat treatment

[0093]

[0094] It can be seen from Table 4 that at 815°C, the transverse elongation after fracture of the heat-treated GH3536 high-temperature alloy material is 42.5%-67.5%, and the longitudinal elongation after fracture is 43.0%-44.5%. Compared with the untreated GH3536 high-temperature alloy material, the transverse and longitudinal elongations of the heat-treated GH3536 high-temperature alloy material at 815°C are greatly improved, which indicates that the toughness of the heat-treated GH3536 high-temperature alloy material is greatly improved.

[0095] In summary, it can be concluded from Tables 2, 3 and 4 that the transverse and longitudinal elongations of the GH3536 high-temperature alloy material at 650°C, 750°C and 815°C are greatly improved after heat treatment, which indicates that the toughness of the material is greatly improved. On the premise that other mechanical properties of the GH3536 high-temperature alloy material meet the requirements, the toughness of the material meets the use requirements.

[0096] The results of the sustained tensile properties at 815° C. of the heat-treated GH3536 high-temperature alloy materials obtained in Examples 1 to 4 and Comparative Examples 1 to 4 and the SLM-formed GH3536 high-temperature alloy materials before heat treatment are shown in Table 5 below.

[0097] Table 5 Test results of the rupture tensile properties of GH3536 superalloy material at 815℃ before and after heat treatment

[0098]

[0099] By comparing the data before and after heat treatment, it can be seen that the transverse endurance time of the GH3536 high-temperature alloy material after heat treatment is 37.5-40.1h, and the transverse elongation is 34%-36%; the longitudinal endurance time is 24-27h, and the longitudinal elongation is 24%-27%. The transverse endurance time and the longitudinal endurance time are significantly improved, the elongation is significantly increased, and the toughness of the material is improved.

[0100] It can be seen from Tables 1 to 5 that the heat-treated GH3536 high-temperature alloy material has excellent comprehensive mechanical properties at room temperature and high temperature conditions, and meets the requirement of high-temperature endurance time ≥ 24h.

[0101] It should be explained that, from the data in Tables 1 to 4, it can be seen that the transverse and longitudinal tensile strength and yield strength of the GH3536 high-temperature alloy material are reduced compared to before heat treatment, and the elongation after fracture is improved, which shows that the plasticity of the GH3536 high-temperature alloy material is improved. This change has different meanings for different application environments of the GH3536 high-temperature alloy material. In addition, the transverse and longitudinal tensile strength and yield strength of the GH3536 high-temperature alloy material after heat treatment by the heat treatment method of the present invention can meet the use requirements. Under this premise, the GH3536 high-temperature alloy material obtains good plasticity (toughness is improved) and has the following uses and meanings:

[0102] First, the forming ability of GH3536 high-temperature alloy material is improved: for applications that require good forming ability (such as deep drawing, bending, etc.), high elongation allows the material to deform better without breaking.

[0103] Secondly, the impact energy absorption of GH3536 high-temperature alloy material is improved: in some cases, the material needs to be able to absorb large impact energy without breaking. For example, using this alloy material with higher elongation in automotive structural parts can absorb more energy during a collision, thereby improving safety.

[0104] Secondly, the welding performance of GH3536 high-temperature alloy material is improved: high elongation helps to improve the stress distribution near the welding area of ​​the alloy material and reduce the risk of crack formation.

[0105] Finally, the anti-brittle fracture performance of the GH3536 high-temperature alloy material has been improved: in low temperature or extremely cold environments, maintaining a certain elongation can prevent the alloy material from becoming too brittle and avoid sudden fracture.

[0106] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A heat treatment method for GH3536 high temperature alloy material, characterized in that: The following steps are involved: Step 1, subjecting the GH3536 high temperature alloy material to hot isostatic pressing treatment, and then cooling it in the furnace; Step 2, homogenizing the GH3536 high temperature alloy material, and then cooling it in the furnace; Step 3: subjecting the GH3536 high temperature alloy material to solid solution treatment, and then cooling it in the furnace to finally obtain the heat-treated GH3536 high temperature alloy material.

2. The heat treatment method of GH3536 high temperature alloy material according to claim 1, characterized in that: In the step 1, the GH3536 high temperature alloy material is a GH3536 high temperature alloy material formed by laser selective melting.

3. The heat treatment method of GH3536 high temperature alloy material according to claim 2, characterized in that: In step 1, the components and mass percentages of the GH3536 high-temperature alloy material formed by laser selective melting are: Cr 19.5%-21.2%, Mo 8.02%-10.4%, Fe17.79%-19.4%, Co 1.32%-1.54%, C 0.11%-0.13%, W0.55%-0.71%, Mn0.02%-0.03%, Si 0.3%-0.35%, and the rest is Ni.

4. The heat treatment method of GH3536 high temperature alloy material according to claim 1, characterized in that: In step 1, during the hot isostatic pressing treatment, the GH3536 high temperature alloy material is first placed in a closed hot isostatic pressing device, and an isotropic pressure of 150 to 170 MPa is applied to the GH3536 high temperature alloy material.

5. The heat treatment method of GH3536 high temperature alloy material according to claim 4, characterized in that: In the step 1, the temperature of the GH3536 high temperature alloy material during hot isostatic pressing is 1150-1250°C.

6. The heat treatment method of GH3536 high temperature alloy material according to claim 5, characterized in that: In the step 1, the GH3536 high temperature alloy material is subjected to hot isostatic pressing for 2 to 4 hours.

7. The heat treatment method of GH3536 high temperature alloy material according to claim 4, characterized in that: In the step 1, the pressure of the GH3536 high temperature alloy material during hot isostatic pressing is 155-165 MPa.

8. The heat treatment method of GH3536 high temperature alloy material according to claim 5, characterized in that: In the step 1, the temperature of the GH3536 high temperature alloy material during hot isostatic pressing is 1180-1220°C.

9. The heat treatment method of GH3536 high temperature alloy material according to claim 6, characterized in that: In the step 1, the GH3536 high temperature alloy material is subjected to hot isostatic pressing for 2.5 to 3.5 hours.

10. A GH3536 high temperature alloy material, characterized in that: The GH3536 high-temperature alloy material is obtained by heat treatment using the heat treatment method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Selective laser melting forming Inconel718 alloy and heat treatment method thereof

    CN111360266A

  • Method for improving durability of GH3536 alloy manufactured by selective laser melting technology

    CN111390180A

  • Heat treatment method of GH3536 high-temperature alloy material formed by SLM (selective laser melting) and application of heat treatment method

    CN114309657A

  • GH3536 raw material powder for laser additive manufacturing, preparation method of GH3536 raw material powder and preparation method of alloy of GH3536 raw material powder

    CN114737083A

  • GH3536 high-temperature alloy powder for laser additive manufacturing and preparation method of GH3536 high-temperature alloy powder

    CN115287501A