Layer forming method and apparatus
By using the combination of molybdenum dichloride dioxide and borohydrogen reactants in the reaction chamber, the problem of poor quality of the molybdenum layer deposition process is solved, and the method of efficient deposition of molybdenum layer in semiconductor devices is realized, which is suitable for molybdenum conductive layer manufacture.
Patent Information
- Application Number
- CN202411239235.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-19
- Filing Date
- 2020-04-14
- Publication Date
- 2024-12-06
AI Technical Summary
The existing molybdenum layer deposition process is poor, and it is difficult to effectively deposit molybdenum layer on the surface of different materials, especially in the manufacturing of semiconductor devices, where there is difficulty in deposition of molybdenum conductive layer.
Use molybdenum dichloride (VI) as a precursor to react with the first reactant containing boron and hydrogen, and form a molybdenum layer through atomic layer deposition (ALD) or chemical vapor deposition (CVD) processes to optimize the deposition process To improve the mass and deposition speed of the molybdenum layer.
Through the improved process method, the deposition quality and speed of the molybdenum layer are significantly improved, and the gaps in semiconductor devices can be effectively filled, which is suitable for the manufacture of high-performance molybdenum conductive layers.
Smart Images

Figure CN119082696A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese invention patent application No. 202010288971.6 filed on April 14, 2020 (applicant: ASM IP Private Holding Co., Ltd., invention name: layer formation method and device). Technical Field
[0002] The present disclosure generally relates to methods and apparatus for forming a layer on a substrate. More particularly, the present disclosure relates to a method and apparatus for depositing a layer comprising molybdenum on a substrate in a reaction chamber.
[0003] The deposition method may include supplying a precursor including molybdenum dioxide dichloride and a first reactant to a substrate in a reaction chamber to react a portion of the precursor with the first reactant to form a molybdenum layer. The layer on the substrate may be used to manufacture a semiconductor device. Background Art
[0004] In atomic layer deposition (ALD) and chemical vapor deposition (CVD), a substrate is subjected to a precursor and a first reactant that are suitable for reacting into a desired layer on the substrate. The layer can be deposited in gaps created during the fabrication of features on the substrate to fill the gaps.
[0005] In ALD, a substrate is exposed to a pulse of a precursor and a monolayer of the precursor may be chemically adsorbed on the surface of the substrate. The surface sites may be occupied by the entire precursor or a fragment of the precursor. The reaction may be chemically self-limiting because the precursor may not adsorb or react with the portion of the precursor that has already been adsorbed on the substrate surface. Excess precursor is then purged, for example, by providing an inert gas and / or removing excess precursor from the reaction chamber with a pump. Subsequently, the substrate is exposed to a pulse of the first reactant, which chemically reacts with the adsorbed entire first precursor or a fragment of the first precursor until the reaction is complete and the surface is covered with a monolayer of reaction products.
[0006] It has been found that there may be a need to improve the quality of the molybdenum layer deposition process. Summary of the invention
[0007] This summary is provided to introduce a series of concepts in a simplified form. These concepts are described in more detail below in the detailed description of the example embodiments of the present disclosure. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0008] Improved methods of forming a deposited molybdenum layer on a substrate may be desired. Therefore, in one embodiment, a method of depositing a layer comprising molybdenum on a substrate in a reaction chamber may be provided. The method may include supplying a precursor comprising molybdenum (VI) dioxide dichloride (MoO2Cl2) to the substrate in the reaction chamber. The method may include supplying a first reactant to the substrate in the reaction chamber to react a portion of the precursor with the first reactant to form the molybdenum layer. The first reactant may include boron and hydrogen.
[0009] By making the first reactant contain boron and hydrogen, the reactivity of the first reactant with the precursor containing molybdenum (VI) dichloride (MoO2Cl2) can be improved. Therefore, the deposition of the molybdenum layer can be improved. The quality of the overall layer can be improved and / or the speed of the deposition process can be improved.
[0010] In some other embodiments, a method for semiconductor processing is provided. The method includes depositing a metal layer into a gap of a substrate, thereby filling the gap.
[0011] According to yet another embodiment, there is provided a deposition apparatus for depositing a layer comprising molybdenum on a substrate, comprising:
[0012] a reaction chamber, wherein the reaction chamber is provided with a substrate holder to hold a substrate;
[0013] a heating system constructed and arranged to control the temperature of the substrate;
[0014] a distribution system comprising a valve for providing a precursor and at least a first reactant in the reaction chamber; and,
[0015] A sequential controller operably connected to the valve and programmed to enable deposition of molybdenum on the substrate in the reaction chamber using the precursor and the first reactant, wherein the distribution system is provided with a precursor delivery device and a first reactant delivery system, the precursor delivery device being used to deliver molybdenum (VI) dichloride (MoO2Cl2) vapor, and the first reactant delivery system being constructed and arranged to deliver vapor of a first reactant comprising boron and hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] While the specification concludes with claims that particularly point out and distinctly claim what are regarded as embodiments of the present invention, advantages of the embodiments of the present disclosure may be more readily ascertained from the description of certain examples of the embodiments of the present disclosure when read in conjunction with the accompanying drawings, in which:
[0017] Figure 1a and 1b A flow chart is shown illustrating a method of depositing a layer according to one embodiment. DETAILED DESCRIPTION
[0018] Although certain embodiments and examples are disclosed below, it will be understood by those skilled in the art that the present invention extends beyond the embodiments and / or applications specifically disclosed herein and their obvious modifications and equivalents. Therefore, it is intended that the scope of the present invention disclosed should not be limited by the specific disclosed embodiments described below.
[0019] The illustrations presented herein are not intended to be actual views of any particular material, structure, or device but are merely idealized illustrations used to describe embodiments of the present disclosure.
[0020] As used herein, the term "substrate" may refer to any underlying material or materials that may be used or upon which a device, circuit, or film may be formed.
[0021] As used herein, the term "cyclic deposition" may refer to the sequential introduction of one or more precursors (reactants) into a reaction chamber to deposit a film over a substrate and includes deposition techniques such as atomic layer deposition and cyclic chemical vapor deposition.
[0022] As used herein, the term "cyclic chemical vapor deposition" may refer to any process in which a substrate is sequentially exposed to one or more volatile precursors that react and / or decompose on the substrate to produce the desired deposition.
[0023] As used herein, the term "atomic layer deposition (ALD)" may refer to a vapor deposition process in which a deposition cycle, preferably a plurality of consecutive deposition cycles, is performed in a processing chamber. Typically, during each cycle, a precursor is chemically adsorbed to a deposition surface (e.g., a substrate surface or a previously deposited underlying surface, such as material from a previous ALD cycle) to form a monolayer or sub-monolayer that is not susceptible to reaction with additional precursors (i.e., a self-limiting reaction). Thereafter, if desired, a reactant (e.g., another precursor or a reactive gas) may subsequently be introduced into the processing chamber for use in converting the chemically adsorbed precursor to the desired material on the deposition surface. Typically, this reactant is capable of further reacting with the precursor. In addition, during each cycle, a purge step may also be utilized to remove excess precursor from the processing chamber after converting the chemically adsorbed precursor and / or to remove excess reactant and / or reaction byproducts from the processing chamber. In addition, the term "atomic layer deposition" as used herein is also intended to include processes designated by related terms such as "chemical vapor atomic layer deposition", "atomic layer epitaxy" (ALE), molecular beam epitaxy (MBE), gas source MBE or organometallic MBE and chemical beam epitaxy when performed using alternating pulses of a precursor composition, a reactive gas, and a purge (e.g., an inert carrier) gas.
[0024] As used herein, the term "layer" may refer to any continuous or non-continuous structure and material formed by the methods disclosed herein. For example, a "layer" may include a 2D material, a nanolaminate, a nanorod, a nanotube, or a nanoparticle, or even a partial or complete molecular layer or a partial or complete atomic layer or a cluster of atoms and / or molecules. A "layer" may include a material or layer with pinholes, but still be at least partially continuous.
[0025] A molybdenum layer may be required as a conductive layer in a semiconductor device. Therefore, a method for depositing a layer comprising molybdenum on a substrate in a reaction chamber may be used. The method may include supplying a precursor comprising molybdenum (VI) dichloride (MoO2Cl2) to the substrate in a reaction chamber. The precursor may include a molybdenum oxyhalide, which is not molybdenum oxytetrachloride (MoOCl4). The precursor may include molybdenum oxychloride, which is not molybdenum oxytetrachloride (MoOCl4). The precursor may have Mo-O and Mo-Cl bonds, which is not molybdenum oxytetrachloride (MoOCl4). The precursor may include a molybdenum oxyhalide having the same number of oxygen as the chlorine atoms bonded to the molybdenum. The precursor may include a molybdenum oxyhalide having two oxygens and two chlorine atoms bonded to the molybdenum.
[0026] The method may further include supplying a first reactant comprising boron and hydrogen to the substrate in the reaction chamber to allow a portion of the precursor to react with the first reactant to form a molybdenum layer on the substrate. The first reactant comprising boron and hydrogen may be selected from the formula B n H (n+x) A borane wherein n is an integer from 1 to 10 and x is an even number.
[0027] The first reactant comprising boron and hydrogen may be selected, for example, from the formula B n H (n+4) of nested boranes.
[0028] The first reactant comprising boron and hydrogen may be selected, for example, from the formula B n H (n+6) of spiderweb borane.
[0029] The first reactant comprising boron and hydrogen may be selected, for example, from the formula B n H (n+8) of open-net borane.
[0030] The first reactant comprising boron and hydrogen may be selected, for example, from the formula B n H m In the above examples, n is an integer from 1 to 10, and m is an integer from 1 to 10 different from n.
[0031] The first reactant comprising boron and hydrogen may be diborane (B2H6). Diborane may have a structure with four terminal hydrogen atoms and two bridging hydrogen atoms. The bond between the boron and terminal hydrogen atoms is a conventional covalent bond. The bonding between the boron atom and the bridging hydrogen atom may be different, because two electrons have been used in the bonding with the terminal hydrogen atoms, and each boron atom has a remaining valence electron to achieve additional bonding. The bridging hydrogen atoms each provide an electron, so the boron atoms in diborane may be held together by four electrons. The length of the BH bridge bond may be longer than the BH terminal bond. This difference in the length of these bonds may reflect the difference in their strength. The BH bridge bond of diborane may be relatively weak.
[0032] The reduction of molybdenum dioxide dichloride (MoO2Cl2) with diborane (B2H6) may have the following reaction path: MoO2Cl2+1 / 2B2H6->Mo(s)+BOCl+HCl+H2O. For this reaction, it may be necessary to break the BH bridge of diborane in order to cut diborane in half. Compared with the reaction path of MoO2Cl2+3H2->Mo(s)+2HCl+2H2O, fewer molecules may be involved, and these molecules may also have weaker hydrogen bonds, which will favor the reaction of MoO2Cl2 with B2H6. The reduction of molybdenum oxychloride (MoOCl4) with diborane (B2H6) will follow MoOCl4+1 / 2B2H6->Mo(s)+BOCl+3HCl, which may cause a higher etchant HCl concentration in the reaction chamber, which may cause undesirable etching and / or reduce deposition rate.
[0033] Diborane can be a highly reactive and versatile reactant. Diborane has been used in the semiconductor industry, for example as a dopant. Therefore, diborane can be easily used in industry as a reactant for molybdenum(VI) dichloride (MoO2Cl2) to deposit molybdenum.
[0034] The surface on which molybdenum may be deposited may comprise one deposition material. Alternatively, the surface may comprise different types of deposition materials. The surface may, for example, comprise aluminum oxide and / or titanium nitride. When, for example, a molybdenum conductive layer is required, it may be difficult to deposit molybdenum on these different materials. The first layer, often referred to as a seed layer or nucleation layer, may be more difficult to deposit. It may therefore be preferred to provide molybdenum (VI) dioxide dichloride (MoO2Cl2) to the substrate in a reaction chamber; and to supply a first reactant comprising boron and hydrogen to the substrate in the reaction chamber so that a portion of the precursor reacts with the first reactant to form a molybdenum seed layer on the substrate.
[0035] The gaps created during the fabrication of features of an integrated circuit device may be filled with a metal layer, for example, made of molybdenum. The gap may have a high aspect ratio because its depth is much greater than its width. The gap may extend vertically in a fabricated layer having a substantially horizontal top surface. Gaps that are vertically and filled with metal may be used, for example, in word lines of memory integrated circuits of the dynamic random access memory (DRAM) type. Gaps that are vertically and filled with metal may also be used, for example, in logic integrated circuits. For example, metal-filled gaps may be used as gate fillers in p-type metal oxide semiconductor (PMOS) or complementary metal oxide semiconductor (CMOS) integrated circuits or source / drain trench contacts.
[0036] The gaps can also be arranged in the horizontal direction in the fabricated layers. Again, the gaps can have a high aspect ratio, since now their depth in the horizontal direction is much larger than their width. Gaps in the horizontal direction and filled with metal can be used, for example, in word lines of 3D NAND type memory integrated circuits. The gaps can also be arranged in a combination of vertical and horizontal directions.
[0037] The surface of the gap may include one type of deposited material. Alternatively, the surface of the gap may include different types of deposited materials. The surface of the gap may, for example, include aluminum oxide and / or titanium nitride. When, for example, a molybdenum conductive layer is required in the gap, it may be difficult to deposit molybdenum on these different materials in the gap. It may be desirable that the molybdenum layer cover the entire surface of the gap and fill the entire gap. In addition, it may be desirable that the molybdenum layer cover the entire surface of the gap including different types of materials.
[0038] In order to fill the entire gap, a molybdenum seed layer may be deposited in the gap and a molybdenum bulk layer may be deposited on the molybdenum seed layer. The seed layer may be formed by sequentially repeating a pretreatment atomic layer deposition (ALD) cycle. Therefore, it may be preferred to provide molybdenum (VI) dioxide (MoO2Cl2) dichloride to the substrate in a reaction chamber; and supply a first reactant comprising boron and hydrogen to the substrate in the reaction chamber to allow a portion of the precursor to react with the first reactant to form a molybdenum seed layer in the gap on the substrate.
[0039] Alternatively, the seed layer may be formed by a chemical vapor deposition (CVD) process. The CVD process may be a pulsed process in which the first precursor is supplied to the substrate in pulses while the first reactant is continuously supplied to the substrate.
[0040] The bulk layer can be deposited on the seed layer by sequentially repeating the bulk ALD cycle. A bulk molybdenum layer can be provided on top of the molybdenum seed layer by supplying a precursor comprising molybdenum (VI) dichloride (MoO2Cl2) and a second reactant comprising hydrogen to the substrate in a reaction chamber, wherein a portion of the precursor reacts with the second reactant to form the bulk molybdenum layer. The second reactant may comprise hydrogen (H2). The second reactant may not comprise boron. Hydrogen may be a relatively cheap and common reactant.
[0041] Alternatively, the bulk molybdenum layer may be deposited on the molybdenum seed layer by a CVD process. The CVD process may be pulsed, where the second precursor is supplied to the substrate in pulses while the second reactant is continuously supplied to the substrate.
[0042] Figure 1a and 1b A flow chart is shown illustrating a method of depositing a molybdenum layer according to one embodiment.
[0043] The molybdenum layer may be deposited as a seed layer. The molybdenum layer may be deposited in the gap. The molybdenum bulk layer may be deposited on the seed layer.
[0044] The first ALD cycle 1 for the Mo seed layer can be Figure 1a The second ALD cycle 2 for the molybdenum bulk layer can be Figure 1b Shown in.
[0045] A substrate having a gap may be provided in the reaction chamber in step 3. A first precursor including molybdenum(VI) dioxide dichloride (MoO2Cl2) may be supplied to the substrate in step 5 for a first supply period T1 (see Figure 1a ). Subsequently, the additional supply of the first precursor to the substrate may be stopped in step 7, for example by purging a portion of the first precursor from the reaction chamber for a first removal period R1.
[0046] In addition, the first cycle may include supplying 9 first reactants to the substrate, continuing the second supply period T2. The first reactant may include boron and hydrogen. The first reactant may include boron and hydrogen atoms in one molecule, for example it may be diborane (B2H6). Hydrogen may be added to the gas stream of the first reactant. A portion of the first precursor and the first reactant may react and form at least a portion of a platinum seed layer on the substrate. Several (about 50) cycles may be required before the deposition of the seed layer is started. The additional supply of the first reactant to the substrate may be stopped in step 10, for example, by purging a portion of the first reactant from the reaction chamber for the second removal period R1.
[0047] Optionally, the first reactant may be used to clean the substrate prior to depositing the seed layer.Diborane reactant may be highly reactive and efficient at cleaning substrate surfaces.
[0048] The first precursor and the first reactant may be selected to have proper nucleation on the surface of the gap. The first ALD cycle 1 may be repeated N times to deposit a molybdenum seed layer, wherein N is selected between 100 and 1000, preferably between 200 and 800, more preferably between 300 and 600. The thickness of the seed layer may be between 1 and 20 nm, preferably between 2 and 10 nm, more preferably between 3 and 7 nm.
[0049] After the first ALD cycle 1 is repeated N times, a first precursor comprising molybdenum(VI) dioxide dichloride (MoO2Cl2) may be supplied to the substrate in step 11 in the bulk ALD cycle 2 for a third supply period T3 (see Figure 1b ). This can be compared with Figure 1a The first ALD cycle 1 is performed in the same reaction chamber or in a different reaction chamber.
[0050] It may be advantageous to perform the bulk ALD cycle in a different reaction chamber than the first ALD cycle when the temperature requirements of the first cycle may be different. A substrate transfer may therefore be required.
[0051] Subsequently, the additional supply of the first precursor to the substrate may be stopped and the substrate removed from the reaction chamber. This may be accomplished by purging a portion of the first precursor from the reaction chamber to the exhaust pump of the reaction chamber in step 13 for a third removal period R3.
[0052] In addition, the cycle may include supplying 15 the second reactant to the substrate for a fourth supply period T4. A portion of the first precursor and the second reactant may react to form at least a portion of the bulk molybdenum layer on the substrate. Additional supply of the second reactant to the substrate may be stopped in step 17, for example, by purging a portion of the second reactant from the reaction chamber for a fourth removal period R4.
[0053] The first precursor and the second reactant may be selected to have appropriate electronic properties. For example, having low resistivity. The resistivity of the molybdenum film may be less than 3000 μΩ-cm, or less than 1000 μΩ-cm, or less than 500 μΩ-cm, or less than 200 μΩ-cm, or less than 100 μΩ-cm, or less than 50 μΩ-cm, or less than 25 μΩ-cm, or less than 15 μΩ-cm or even less than 10 μΩ-cm.
[0054] The second ALD cycle 2 of the bulk layer may be repeated M times, wherein M is selected between 200 and 2000, preferably between 400 and 1200, more preferably between 600 and 1000. The thickness of the bulk molybdenum layer may be between 1 and 100 nm, preferably between 5 and 50 nm, more preferably between 10 and 30 nm.
[0055] The process temperature during the first ALD cycle of the seed molybdenum layer may be between 300 and 800° C., preferably between 400 and 700° C., more preferably between 500 and 650° C. The container in which the first precursor is vaporized may be maintained between 20 and 150° C., preferably between 30 and 120° C., more preferably between 40 and 110° C.
[0056] The process temperature during the second ALD cycle of the bulk molybdenum layer may be between 300 and 800° C., preferably between 400 and 700° C., more preferably between 500 and 650° C. The container in which the first precursor is vaporized may be maintained between 20 and 150° C., preferably between 30 and 120° C., more preferably between 40 and 110° C.
[0057] Supplying the first precursor into the reaction chamber may take a duration T1, T3 selected between 0.1 and 10 seconds, preferably between 0.5 and 5 seconds, more preferably between 0.8 and 2 seconds. For example, T1 may be 1 second and T3 may be 1.3 seconds. The flow rate of the first or second precursor into the reaction chamber may be selected between 50 and 1000 sccm, preferably 100 and 500 sccm, and more preferably 200 and 400 sccm. The pressure in the reaction chamber may be selected between 0.1 and 100 Torr, preferably 1 and 50 Torr, and more preferably 4 and 20 Torr.
[0058] Supplying the first and / or second reactant to the reaction chamber over duration T2, T4 may take between 0.5 and 50 seconds, preferably between 1 and 10 seconds, and more preferably between 2 and 8 seconds. The flow rate of the first or second reactant to the reaction chamber may be between 50 and 50,000 sccm, preferably between 100 and 20,000 sccm, and more preferably between 500 and 10,000 sccm.
[0059] As the second reactant, silane can also be considered. The general formula of silane is Si x H 2(x+2) , wherein x is an integer of 1, 2, 3, 4, ... Silane (SiH4), disilane (Si2H6) or trisilane (Si3H8) may be suitable examples of the second reactant having a hydrogen atom.
[0060] The duration R1, R2, R3 or R4 for which a portion of at least one of the first precursor, the first reactant and the second reactant is purged from the reaction chamber may be selected between 0.5 and 50 seconds, preferably between 1 and 10 seconds, more preferably between 2 and 8 seconds.
[0061] Purging can be used to remove a portion of at least one of the first precursor, the first reactant, and the second reactant from the reaction chamber for a duration of R1, R2, R3, or R4 after supplying the first precursor to the substrate; after supplying the first reactant to the substrate; and after supplying the second reactant to the reaction chamber. Purging can be achieved by pumping and / or by providing a purge gas. The purge gas can be an inert gas such as nitrogen.
[0062] The method can be used in single wafer or batch wafer ALD equipment.
[0063] The method may include providing a substrate in a reaction chamber and a first ALD cycle in the reaction chamber may include: supplying a first precursor to the substrate in the reaction chamber; purging a portion of the first precursor from the reaction chamber; supplying a first reactant to the substrate in the reaction chamber; and purging a portion of the first reactant from the reaction chamber.
[0064] Additionally, the method may include providing a substrate in a reaction chamber and a bulk ALD cycle in the reaction chamber may include: supplying a second precursor to the substrate in the reaction chamber; purging a portion of the second precursor from the reaction chamber; supplying a second reactant to the substrate in the reaction chamber; and purging a portion of the second reactant from the reaction chamber.
[0065] An exemplary single wafer reactor specifically designed for performing an ALD process is available under the trade name and Commercially available from ASM International NV (Almere, The Netherlands). The method can also be performed in a batch wafer reactor, such as a vertical furnace. For example, the deposition method can also be performed in an A400 TM or A412 TM The furnace may have a process chamber that can accommodate a load of more than 100 semiconductor substrates or wafers with a diameter of 200 or 300 mm.
[0066] The wafer reactor may have a controller and a memory that can control the reactor. The memory may be programmed to supply precursors and reactants in the reaction chamber according to embodiments of the present disclosure when executed on the controller.
[0067] The gaps that can be filled with platinum using the methods of the present disclosure can have a high aspect ratio because the vertical and / or horizontal depth is much greater than the width. For example, the aspect ratio of the gap (gap depth / gap width) can be greater than about 2, greater than about 5, greater than about 10, greater than about 20, greater than about 50, greater than about 75, or even greater than about 100, or greater than about 150, or greater than about 200 in some cases. The aspect ratio can be less than 1000.
[0068] It may be noted that it may be difficult to determine the aspect ratio for the gaps, but in this case, the aspect ratio may be replaced by the surface enhancement ratio, which may be the ratio of the total surface area of the gaps in the wafer or a portion of the wafer relative to the planar surface of the wafer or a portion of the wafer. The surface enhancement ratio of the gaps (surface gaps / surface wafer) may be greater than about 2, greater than about 5, greater than about 10, greater than about 20, greater than about 50, greater than about 75, or even greater than about 100, or greater than about 150, or greater than about 200 in some cases. The surface enhancement ratio may be less than 1000.
[0069] The surface of the gap may comprise different kinds of deposited materials. The surface may comprise Al2O3 or TiN, for example.
[0070] By repeating a first ALD cycle sequentially with a first precursor and a first reactant to deposit a seed layer, a conformal molybdenum metal layer can be deposited on the surface of the gap. In addition, by repeating a second ALD cycle sequentially with a first precursor and a second reactant, a conformal molybdenum bulk layer can be deposited on the seed layer.
[0071] Details of the method used are shown in Figures 1 and 1b and the associated description. In some embodiments, the step coverage of the deposited film including Mo can be greater than about 50%, greater than about 80%, greater than about 90%, greater than about 95%, greater than about 98%, greater than about 99%.
[0072] The method may be performed in an atomic layer deposition apparatus. For example, a deposition apparatus for depositing a layer comprising molybdenum on a substrate may include:
[0073] a reaction chamber, wherein the reaction chamber is provided with a substrate holder to hold a substrate;
[0074] a heating system constructed and arranged to control the temperature of the substrate;
[0075] a distribution system comprising a valve for providing a precursor and at least a first reactant in the reaction chamber; and,
[0076] A sequence controller is operably connected to the valve and programmed to enable deposition of molybdenum on a substrate in a reaction chamber using a precursor and a first reactant.
[0077] The distribution system may be provided with a precursor delivery device and a first reactant delivery system, wherein the precursor delivery device is constructed and arranged to deliver molybdenum (VI) dichloride (MoO2Cl2) vapor, and the first reactant delivery system is constructed and arranged to deliver vapor of a first reactant comprising boron and hydrogen, such as diborane.
[0078] The first reactant may be diborane and may be supplied in the reaction chamber for a duration T2, T4 of 5 seconds at a flow rate between 50 and 50,000 sccm, for example 495 sccm. After supplying the first precursor; after supplying the first precursor and after supplying the first reactant; a nitrogen purge gas may be used for a duration R1, R2, R3 or R4 of 5 seconds.
[0079] During the pre-treatment and bulk ALD cycles, the process temperature may be, for example, about 550°C and the pressure may be about 10 Torr. The container in which the first precursor may be vaporized may be about 70°C.
[0080] The method can also be used in a spatial atomic layer deposition device. In spatial ALD, precursors and reactants are continuously supplied in different physical sections and the substrate moves between sections. At least two sections can be provided in which half reactions can be performed in the presence of a substrate. If a substrate is present in such a half-reaction section, a monolayer can be formed from the first or second precursor. Then, the substrate is moved to the second half-reaction zone, where the ALD cycle is completed by the first or second reactant to form an ALD monolayer. Alternatively, the substrate position can be fixed and the gas supply can be movable, or some combination of the two. To obtain a thicker film, this process can be repeated.
[0081] According to one embodiment of a spatial ALD apparatus, a method comprises:
[0082] placing a substrate in a reaction chamber comprising a plurality of sections, each section being separated from an adjacent section by a gas curtain;
[0083] supplying a first precursor, such as molybdenum(VI)dichloride, to a substrate in a first section of a reaction chamber;
[0084] moving the substrate surface relative to the reaction chamber (e.g., laterally) through the gas curtain to a second section of the reaction chamber;
[0085] supplying a first reactant (e.g., diborane) comprising boron and hydrogen to the substrate in a second section of the reaction chamber to form a molybdenum seed layer;
[0086] moving the substrate surface relative to the reaction chamber (e.g., laterally) across the gas curtain; and
[0087] The first precursor and the reactant are repeatedly supplied, including moving the substrate surface relative to the reaction chamber (eg, laterally) to form a molybdenum seed layer.
[0088] To form the bulk layer, the method may further include:
[0089] placing a substrate in a reaction chamber comprising a plurality of sections, each section being separated from an adjacent section by a gas curtain;
[0090] supplying a first precursor, such as molybdenum(VI)dichloride, to a substrate in a first section of a reaction chamber;
[0091] moving the substrate surface relative to the reaction chamber (e.g., laterally) through the gas curtain to a second section of the reaction chamber;
[0092] supplying a second reactant, such as hydrogen (H2), to the substrate in a second section of the reaction chamber to form a bulk layer of molybdenum;
[0093] Moving the substrate surface relative to the reaction chamber (e.g., laterally) through the gas curtain; and, repeatedly supplying the first precursor and the second reactant, including moving the substrate surface relative to the reaction chamber (e.g., laterally) to form a molybdenum bulk layer.
[0094] The first reactant may include hydrogen and boron, such as diborane. The second reactant may be hydrogen (H2).
[0095] In other embodiments, the seed or bulk molybdenum layer may contain less than about 40 atomic %, less than about 30 atomic %, less than about 20 atomic %, less than about 10 atomic %, less than about 5 atomic %, or even less than about 2 atomic % oxygen. In further embodiments, the seed or bulk layer may contain less than about 30 atomic %, less than about 20 atomic %, less than about 10 atomic %, less than about 5 atomic %, or less than about 2 atomic %, or even less than about 1 atomic % hydrogen.
[0096] In some embodiments, the seed or bulk molybdenum layer may contain less than about 10 atomic %, or less than about 5 atomic %, less than about 1 atomic %, or even less than about 0.5 atomic % of halogen or chlorine. In still further embodiments, the seed or bulk molybdenum layer may contain less than about 10 atomic %, or less than about 5 atomic %, or less than about 2 atomic %, or less than about 1 atomic %, or even less than about 0.5 atomic % of carbon. In the embodiments outlined herein, the atomic percentage (at. %) concentration of an element may be determined using Rutherford backscattering (RBS).
[0097] In some embodiments of the present disclosure, forming a semiconductor device structure, such as a semiconductor device structure, may include forming a gate electrode structure including a molybdenum film, the effective work function of the gate electrode structure being greater than about 4.9 eV, or greater than about 5.0 eV, or greater than about 5.1 eV, or greater than about 5.2 eV, or greater than about 5.3 eV, or even greater than about 5.4 eV. In some embodiments, an electrode structure including a molybdenum layer having a thickness of less than about 100 angstroms, or less than about 50 angstroms, or less than about 40 angstroms, or even less than about 30 angstroms may exhibit the effective work function values given above.
[0098] It will be appreciated by those skilled in the art that various omissions, additions, and modifications may be made to the methods and structures described above without departing from the scope of the present invention. It is contemplated that various combinations or sub-combinations of the specific features and aspects of the embodiments may be made and still fall within the scope of the description. The various features and aspects of the disclosed embodiments may be sequentially combined or substituted with one another. As defined by the appended claims, all such modifications and variations are intended to fall within the scope of the present invention.
Claims
1. A method of depositing a layer comprising molybdenum on a substrate in a reaction chamber, the method comprising: Forming a seed layer includes the following steps: supplying a precursor comprising molybdenum(VI) dioxide dichloride (MoO2Cl2) to the substrate in the reaction chamber; and, supplying a first reactant to the substrate in the reaction chamber to allow a portion of the precursor to react with the first reactant to form the seed layer, wherein the first reactant comprises boron and hydrogen (H2); and Forming the body layer comprises the following steps: supplying the precursor comprising molybdenum(VI) dioxide dichloride (MoO2Cl2) to the substrate in the reaction chamber; and, A second reactant including hydrogen is supplied to the substrate in the reaction chamber, wherein a portion of the precursor reacts with the second reactant to form the bulk molybdenum layer.
2. The method according to claim 1, wherein: The seed layer is formed by atomic layer deposition.
3. The method according to claim 2, wherein: The bulk molybdenum layer is formed by chemical vapor deposition.
4. The method according to claim 1, wherein: The surface of the substrate includes aluminum oxide and / or titanium nitride.
5. The method according to claim 1, wherein: The precursor is supplied to the reaction chamber in pulses and the pulses are between 0.1 and 10 seconds. The method of claim 1 , wherein the flow rate of the precursor into the reaction chamber is between 50 and 1000 sccm. 7 . The method of claim 1 , wherein the flow rate of the first reactant into the reaction chamber is between 50 and 50,000 sccm.
8. The method of claim 1, wherein the pressure in the reaction chamber is between 0.1 and 100 Torr.
9. The method according to claim 1, wherein the deposition process temperature is between 300 and 800°C.
10. The method of claim 1, wherein depositing the molybdenum layer comprises repeating an atomic layer deposition (ALD) cycle including sequentially supplying the precursor and the first reactant to the substrate. The method of claim 10 , wherein the substrate is purged for 0.5 to 50 seconds between supplying the precursor and the first reactant.
12. The method of claim 11, wherein supplying the first reactant into the reaction chamber takes between 0.5 and 50 seconds.
13. The method according to claim 1, wherein: The first reactant comprising boron and hydrogen is selected from boranes of the formula BnH(n+x), wherein n is an integer from 1 to 10 and x is an even number.
14. The method of claim 13, wherein the first reactant comprising boron and hydrogen is selected from the group consisting of: n H (n+4) of nested boranes.
15. The method of claim 13, wherein the first reactant comprising boron and hydrogen is selected from the group consisting of: n H (n+6) of spiderweb borane.
16. The method of claim 13, wherein the first reactant comprising boron and hydrogen is selected from the group consisting of: n H (n+8) of open-net borane.
17. The method of claim 1, wherein the surface comprises a gap, wherein surfaces of the gap comprise different materials.
18. The method of claim 1, wherein the first reactant comprising boron and hydrogen is selected from the group consisting of biborane B n H m , wherein n is an integer from 1 to 10, and m is an integer from 1 to 10 different from n.
19. The method of claim 1, wherein the first reactant comprising boron and hydrogen is provided in the reaction chamber to prepare a surface of the substrate before providing the precursor to the reaction chamber.
20. The method of claim 1, wherein the substrate comprises one or more gaps created during fabrication of features on the substrate and the one or more gaps are at least partially filled by the method of depositing a layer comprising molybdenum on the substrate in a reaction chamber.
Citation Information
Patent Citations
Methods for depositing molybdenum metal film over dielectric surface of substrate by cyclical deposition process and related semiconductor device structures