Surface passivation auxiliary growth method of two-dimensional ultrathin non-layered material beta-Bi2O3 and application of two-dimensional ultrathin non-layered material beta-Bi2O3 in photoelectric field

By using Bi2Se3 auxiliary agent on the surface of the two-dimensional non-layered material β-Bi2O3, it inhibits its vertical growth, and realizes the synthesis of ultra-thin and large-size non-layered material, solving the problem of growth in the prior art, supporting High-performance optoelectronics applications.

CN119082700AActive Publication Date: 2024-12-06TIANJIN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411199466.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The prior art is difficult to balance the growth of its ultra-thin thickness and large-size crystals when synthesizing two-dimensional non-layered materials, resulting in limited performance and device integration.

Method used

Bi2Se3 is used as an auxiliary agent to react with the β-Bi2O3 surface at high temperature by vapor deposition method, inhibit its vertical growth and promote lateral growth, thereby obtaining an ultra-thin and large-size two-dimensional non-layered material β-Bi2O3.

Benefits of technology

The controllable synthesis of the non-layered material β-Bi2O3 with high quality, ultra-thin thickness and large transverse size is achieved, supporting the application of high-performance devices, and simplifying the preparation process, avoiding the upgrading and transformation of traditional CVD systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082700A_ABST
    Figure CN119082700A_ABST
Patent Text Reader

Abstract

The invention discloses a surface passivation auxiliary growth method of a two-dimensional ultrathin non-layered material beta-Bi2O3 and application of the two-dimensional ultrathin non-layered material beta-Bi2O3 in the photoelectric field, and belongs to the technical field of two-dimensional non-layered materials and photoelectric materials. According to the preparation method, Bi2O3 is taken as a precursor, Bi2Se3 is taken as an auxiliary agent, Se atoms volatilized from Bi2Se3 at a high temperature can be bonded with unsaturated Bi atoms on the surface of a beta-Bi2O3 sheet, the surface of beta-Bi2O3 is passivated, growth of beta-Bi2O3 in the vertical direction is inhibited, transverse growth of beta-Bi2O3 is promoted, and the ultrathin large-size non-layered beta-Bi2O3 crystal can be obtained. The preparation method is high in controllability, the problem that the thickness of the non-layered material is uncontrollable can be well solved, and the non-layered material with the ultra-thin thickness and the large transverse size can be obtained easily.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of two-dimensional non-layered materials and optoelectronic materials, and in particular relates to a surface passivation-assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 and its application in the optoelectronic field. Background Art

[0002] In recent years, two-dimensional materials have attracted increasing attention in the fields of electronics, optoelectronics, energy storage and conversion due to their excellent performance and broad application prospects. Among them, two-dimensional non-layered materials have abundant surface dangling bonds and highly active surfaces, showing superior performance, and are an indispensable extension and supplement to two-dimensional layered materials. First, the ultra-thin thickness gives two-dimensional non-layered materials excellent optical transparency, significant flexibility and mechanical strength, making them promising candidates for the manufacture of flexible devices. In addition, ultra-thin non-layered materials have tunable band gaps and enhanced conductivity, as well as ultra-high specific surface area, which promotes their application in high-performance electronics and optoelectronics. Therefore, the synthesis of two-dimensional ultra-thin non-layered materials has important basic research and practical technical significance.

[0003] Currently, researchers have also developed some methods for synthesizing two-dimensional non-layered materials, such as salt-assisted chemical vapor deposition and spatial confinement. Although significant progress has been made in this field, challenges still exist in balancing the ultra-thin thickness and extended crystal size of non-layered materials and in the synthesis of other two-dimensional non-layered materials. This is mainly because non-layered materials have intrinsic isotropic chemical bonds in all directions, making their two-dimensional anisotropic growth very challenging, which in turn limits the exploration of their performance and device integration.

[0004] Therefore, a new growth method is urgently needed to promote the ultrathin growth of non-layered materials, so as to realize the synthesis of ultrathin and large-sized non-layered materials. Summary of the Invention

[0005] In order to solve the above technical problems, the present invention proposes a surface passivation-assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 and its application in the optoelectronic field.

[0006] To achieve the above objectives, the present invention provides the following technical solutions:

[0007] The present invention provides a surface passivation-assisted growth method for two-dimensional ultrathin non-layered material β-Bi2O3, comprising the following steps: using Bi2O3 as a precursor and Bi2Se3 as an auxiliary agent to obtain the two-dimensional ultrathin non-layered material β-Bi2O3 through vapor deposition.

[0008] Preferably, the mass ratio of Bi2O3 to Bi2Se3 is 2:1.

[0009] Preferably, the vapor deposition includes the following steps: placing Bi2O3 and Bi2Se3 at the heat source center and upstream of the tubular furnace respectively, placing fluorophlogopite directly above Bi2O3, then heating to the growth temperature for crystal growth, and then cooling to room temperature to obtain the two-dimensional ultra-thin non-layered material β-Bi2O3.

[0010] Preferably, the distance between the fluorphlogopite and Bi2O3 is 4 mm.

[0011] Preferably, the fluorophlogopite further includes a pre-treatment step before use; the pre-treatment method is: peeling the fluorophlogopite and using the freshly dissociated surface as the crystal growth surface.

[0012] Preferably, the growth temperature is 680-750°C.

[0013] Preferably, the crystal growth time is 20-60 min.

[0014] The present invention provides a two-dimensional ultra-thin non-layered material β-Bi2O3 obtained by the surface passivation assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 described in the above technical solution.

[0015] Preferably, the thinnest thickness of the two-dimensional ultra-thin non-layered material β-Bi2O3 is 0.77 nm, and the maximum lateral dimension is 163 μm.

[0016] The present invention also provides the application of the two-dimensional ultra-thin non-layered material β-Bi2O3 described in the above technical solution in the optoelectronic field.

[0017] Compared with the prior art, the present invention has the following advantages and technical effects:

[0018] 1. The present invention uses Bi2Se3 as an auxiliary agent. The Se atoms volatilized at high temperature can bond with the unsaturated Bi atoms on the surface of the β-Bi2O3 flakes, thereby passivating the surface of β-Bi2O3, inhibiting its vertical growth and promoting lateral growth, thus facilitating the acquisition of ultra-thin, large-sized, non-layered β-Bi2O3 crystals.

[0019] 2. The preparation method provided by the present invention is efficient and convenient, with a simple device. There is no need to upgrade or modify the traditional CVD system. Ultra-thin, large-sized non-layered β-Bi2O3 crystals can be obtained by simply adding Bi2Se3 sheets as an auxiliary agent during the growth process.

[0020] 3. The preparation method provided by the present invention has high controllability and can effectively solve the problem of uncontrollable thickness of non-layered materials. It is conducive to obtaining non-layered materials with ultra-thin thickness and large lateral size, laying a solid foundation for the application of high-performance devices based on non-layered β-Bi2O3 crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings, which constitute part of this application, are intended to provide a further understanding of this application. The exemplary embodiments and descriptions of this application are intended to explain this application and do not constitute an improper limitation on this application. In the accompanying drawings:

[0022] Figure 1 Schematic diagram of the positional relationship between the precursor and the auxiliary agent in the surface passivation-assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 provided by the present invention;

[0023] Figure 2 Schematic diagram of the crystal growth process of the surface passivation-assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 provided by the present invention;

[0024] Figure 3 Optical microscope images (ab) of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1, optical microscope image (c) of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 2, atomic force microscope image (d) of β-Bi2O3, Raman spectrum (e) and Raman scan of characteristic peaks (f);

[0025] Figure 4 High-angle annular dark-field scanning transmission electron microscopy image of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1 (a), an enlarged view of Figure a (b), an intensity line profile extracted from the white dashed box in Figure b (c), a selected area electron diffraction pattern of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1 (d), an atomic model of the β-Bi2O3 crystal along the (100) direction (e), the adsorption energy of Se atoms on different surfaces of β-Bi2O3 (f), and the adsorption energy of Se atoms from the internal bulk phase of β-Bi2O3 to the surface atomic layer (gh);

[0026] Figure 5 Optical microscope images of β-Bi2O3 prepared in Example 1 and Comparative Examples 1-3;

[0027] Figure 6 Schematic diagram of the structure of the photodetector prepared in Example 3 (a), IV curves under different light intensities (b), intensity-dependent responsivity and detectivity (c), EQE under different light intensities (d), IT curves under different wavelengths (e), and characteristic light response time curve in fast scanning mode (f);

[0028] Figure 7 Schematic diagram of the structure of the polarization-sensitive photodetector prepared in Example 4 (a), the IV curve under periodic change of polarization angle (b), the polar coordinate diagram of polarization-dependent photocurrent (c), and the polar coordinate diagram of polarization-dependent responsivity (d). DETAILED DESCRIPTION

[0029] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] An embodiment of the present invention provides a surface passivation-assisted growth method for a two-dimensional ultra-thin non-layered material β-Bi2O3, comprising the following steps: using Bi2O3 as a precursor and Bi2Se3 as an auxiliary agent, and obtaining a two-dimensional ultra-thin non-layered material β-Bi2O3 by vapor deposition.

[0032] The present invention adds Bi2Se3 as an auxiliary agent to inhibit the vertical growth of β-Bi2O3 and promote its lateral growth, thereby obtaining high-quality non-layered material β-Bi2O3 with ultra-thin thickness and large lateral size.

[0033] In a preferred embodiment, the mass ratio of Bi2O3 to Bi2Se3 is 2: 1. The amount of the auxiliary agent Bi2Se3 used in the present invention affects the passivation effect, thereby affecting the growth behavior of β-Bi2O3. By controlling the amount of the auxiliary agent, the controllable preparation of large-area ultra-thin β-Bi2O3 is achieved.

[0034] In a preferred embodiment, the Bi2O3 is in powder form, has an α-type crystal structure, and has a purity of not less than 99.999%; the Bi2Se3 is in flake form, and has a purity of not less than 99.999%.

[0035] In a preferred embodiment, the vapor deposition process includes the following steps: placing Bi2O3 and Bi2Se3 at the center and upstream of a heat source in a tube furnace, respectively; placing fluorphlogopite directly above the Bi2O3; then heating the furnace to the growth temperature for crystal growth; and subsequently cooling the furnace to room temperature to produce the two-dimensional, ultra-thin, non-layered β-Bi2O3 material. During crystal growth, the Bi2O3 precursor adsorbs on the fluorphlogopite surface to form nuclei and epitaxial growth, while the auxiliary agent Bi2Se3 adsorbs on the exposed surfaces of the β-Bi2O3 flakes, inhibiting their vertical growth and promoting their lateral growth.

[0036] In a preferred embodiment, the distance between the center of the heat source and the upstream is 4 cm.

[0037] In a preferred embodiment, the distance between the fluorphlogopite and Bi2O3 is 4 mm.

[0038] In a preferred embodiment, the fluorophlogopite mica further includes a pretreatment step before use. The pretreatment method includes exfoliating the fluorophlogopite mica, using the freshly dissociated surface as the crystal growth surface. The fluorophlogopite mica has a size of 1 cm x 1 cm, and the tools used for exfoliation are precision tweezers and tape. The present invention uses fluorophlogopite as a substrate, which has the advantage of being atomically flat, facilitating the growth of non-layered materials.

[0039] In a preferred embodiment, the fluorophlogopite is in the form of a sheet and the number is one sheet.

[0040] In a preferred embodiment, the growth temperature is 680-750°C. Controlling the growth temperature within this range facilitates obtaining Bi2O3 with a β-type crystal structure. Furthermore, at this temperature, both the precursor and the auxiliary agent evaporate, allowing the precursor Bi2O3 to adsorb on the fluorphlogopite surface to form nuclei and epitaxial growth, while the auxiliary agent Bi2Se3 adsorbs on the exposed surface of the β-Bi2O3 flakes, inhibiting their vertical growth and promoting their lateral growth.

[0041] In a preferred embodiment, the heating rate of heating to the growth temperature is 16° C. / min.

[0042] In a preferred embodiment, the crystal growth time is 20-60 minutes. In the present invention, the crystal growth time affects the size of the final product. By controlling the crystal growth time, the controllable preparation of large-area ultra-thin β-Bi2O3 is achieved.

[0043] In a preferred embodiment, the cooling rate to room temperature is 12°C / min.

[0044] In a preferred embodiment, the vapor deposition uses Ar gas as a carrier gas for transporting gas; the flow rate of the Ar gas is 50-80 sccm.

[0045] The present invention provides a two-dimensional ultra-thin non-layered material β-Bi2O3 obtained by the surface passivation assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 described in the above technical solution.

[0046] In a preferred embodiment, the thinnest thickness of the two-dimensional ultra-thin non-layered material β-Bi2O3 is 0.77 nm, and the maximum lateral dimension is 163 μm.

[0047] The two-dimensional ultra-thin non-layered material β-Bi2O3 provided by the present invention has an ultra-thin thickness and a large lateral size.

[0048] The present invention also provides the application of the two-dimensional ultra-thin non-layered material β-Bi2O3 described in the above technical solution in the optoelectronic field.

[0049] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0050] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0051] Example 1

[0052] The surface passivation-assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 has the following specific steps:

[0053] S1. Use freshly peeled fluorophlogopite with a size of 1 cm×1 cm as the growth substrate.

[0054] S2. Use Bi2O3 powder with a purity of not less than 99.999% as a precursor and Bi2Se3 flakes with a purity of not less than 99.999% as an auxiliary agent.

[0055] S3. Weigh 60 mg of α-Bi2O3 powder and 30 mg of Bi2Se3 flakes, and place them at the center and upstream of the heat source of the tube furnace, respectively. At the same time, place the fresh fluorphlogopite prepared in step S1 4 mm above the Bi2O3 powder.

[0056] S4. The tube furnace was heated at a heating rate of 16°C / min from room temperature to 700°C, and Ar gas was used as a carrier gas with a flow rate of 50 sccm.

[0057] S5. Maintain the temperature at 700°C for 20 minutes for crystal growth, and then cool the system temperature to room temperature at a cooling rate of 12°C / min in an Ar atmosphere to obtain a two-dimensional ultra-thin non-layered material β-Bi2O3.

[0058] Figure 1 This is a schematic diagram of the positional relationship between the precursor and the auxiliary agent in the surface passivation-assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 provided by the present invention, wherein the yellow is Bi2O3 powder, the green is Bi2Se3 flakes, and the pink is fluorphlogopite. Figure 1 It can be seen that the Bi2O3 powder is located at the heat source center of the tube furnace, the Bi2Se3 sheet is located upstream of the tube furnace, and the fluorphlogopite is located just above the Bi2O3 powder.

[0059] Figure 2 Schematic diagram of the crystal growth process of the surface passivation assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 provided by the present invention. Figure 2It can be seen that when Bi2Se3 is used as an auxiliary agent, the adsorption and growth of Bi2O3 in the vertical direction can be inhibited, making it more inclined to adsorb and grow along the lateral direction, which is conducive to obtaining ultra-thin Bi2O3.

[0060] Figure 3 The optical microscope images (ab) of the two-dimensional ultra-thin non-layered material β-Bi2O3 prepared in Example 1, the optical microscope image (c), atomic force microscope image (d), Raman spectrum (e) and Raman scan of characteristic peaks (f) of the two-dimensional ultra-thin non-layered material β-Bi2O3 prepared in Example 2. Figure 3 As can be seen from the ab part, the maximum lateral dimension of the two-dimensional ultra-thin non-layered material β-Bi2O3 prepared in Example 1 can reach 163 μm, and has an ultra-thin thickness. Figure 3 As can be seen from the middle d part, its thinnest thickness is as low as 0.77nm. Figure 3 The middle e part shows the characteristic peak of β-Bi2O3, which confirms the successful synthesis of β-Bi2O3. -1 The characteristic peaks of the Raman scan are shown in the following figure. Figure 3 As shown in part f, the signal intensity distribution is uniform across the entire sample area, confirming that the synthesized β-Bi2O3 flakes are of high quality.

[0061] Figure 4 The high-angle annular dark field scanning transmission electron microscopy image (a) of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1, the enlarged view of Figure a (b), the intensity line profile extracted from the white dotted box in Figure b (c), the selected area electron diffraction pattern of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1 (d), the atomic model of the β-Bi2O3 crystal along the (100) direction (e), the adsorption energy of Se atoms on different surfaces of β-Bi2O3 (f), and the adsorption energy of Se atoms from the internal bulk phase of β-Bi2O3 to the surface atomic layer (gh). Figure 4 As can be seen from part a, the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 1 presents a highly ordered atomic structure arrangement and no obvious defects, which proves that the synthesized Bi2O3 crystals have high crystalline quality. The measured lattice spacing is 0.77nm and 0.58nm, corresponding to the (010) and (001) crystal planes of β-Bi2O3, respectively. Figure 4 Part b further presents the magnified high-angle annular dark-field scanning transmission electron microscopy image, which is similar to the Figure 4 Part e is consistent with the crystal structure model observed from the (100) direction of Bi2O3. Figure 4 The red box in b is a typical unit cell, which is also Figure 4 The unit cells in e fit perfectly. Figure 4Part c clearly shows the consistent intensity of each Bi atomic column, confirming that the synthesized β-Bi2O3 is of high quality and excellent uniformity. Figure 4 The selected area electron diffraction pattern in part d shows a single set of diffraction spots, which is consistent with the lattice characteristics of β-Bi2O3 and confirms the single crystal characteristics of the synthesized β-Bi2O3. Figure 4 Part f shows the adsorption energy of Se on the (100), (011) and (111) surfaces of β-Bi2O3 crystals. Se atoms preferentially bond with unsaturated Bi atoms to form Bi-Se order. The adsorption energy of Se on the (100) surface is 0.30 eV, while the adsorption energy of Se on the (011) and (111) surfaces is 1.11 eV and 1.54 eV respectively. By comparison, it is found that the adsorption energy of Se on the (100) surface is significantly lower. Figure 4 As can be seen in the middle gh part, for the (100) plane, the adsorption energy of Se atoms gradually decreases from the internal bulk phase to the surface atomic layer of β-Bi2O3. These results demonstrate that Se atoms preferentially adsorb on the (100) surface of β-Bi2O3 and occupy surface sites, thereby inhibiting growth in the vertical direction and promoting the growth of ultrathin β-Bi2O3.

[0062] Example 2

[0063] The difference from Example 1 is that in step S5, the crystal growth is carried out by maintaining the temperature at 700° C. for 60 minutes, and the remaining steps are the same as Example 1.

[0064] Figure 3 Part c is an optical microscope image of the two-dimensional ultrathin non-layered material β-Bi2O3 prepared in Example 2. It can be seen that large-area β-Bi2O3 crystals can be obtained under the condition of a crystal growth time of 60 minutes.

[0065] Comparative Example 1

[0066] The difference from Example 1 is that the Bi2Se3 sheet is omitted, and the remaining steps are the same as Example 1.

[0067] Comparative Example 2

[0068] The difference from Example 1 is that in step S3, 60 mg of Bi2O3 powder and 60 mg of Bi2Se3 flakes are weighed, and the remaining steps are the same as in Example 1.

[0069] Comparative Example 3

[0070] The difference from Example 1 is that in step S3, 60 mg of Bi2O3 powder and 20 mg of Bi2Se3 flakes are weighed, and the remaining steps are the same as in Example 1.

[0071] Figure 5The optical microscope images of β-Bi2O3 prepared in Example 1 and Comparative Examples 1-3 are shown, where a is Comparative Example 1 (Bi2O3:Bi2Se3=1:0), b is Comparative Example 2 (Bi2O3:Bi2Se3=1:1), c is Example 1 (Bi2O3:Bi2Se3=2:1), and d is Comparative Example 3 (Bi2O3:Bi2Se3=3:1). Figure 5 As can be seen from part a, without adding auxiliary agent Bi2Se3, the obtained β-Bi2O3 has a large thickness. Figure 5 As can be seen in part b, when the mass ratio of Bi2O3 to Bi2Se3 is 1:1, irregular dots are grown, and there is no synthesis of β-Bi2O3 products with two-dimensional morphology. Figure 5 As can be seen from part d, when the mass ratio of Bi2O3 to Bi2Se3 is 3:1, the grown β-Bi2O3 has a large thickness, and it is difficult to synthesize β-Bi2O3 with ultra-thin thickness.

[0072] Example 3

[0073] The two-dimensional ultra-thin non-layered material β-Bi2O3 prepared in Example 1 was made into a photodetector. The structure of the photodetector is shown in FIG. Figure 6 In a, the specific preparation process is as follows: the device is prepared based on the two-dimensional ultra-thin non-layered material β-Bi2O3 synthesized in Example 1, and electrodes formed by 10 nm thick Cr and 30 nm thick Au are transferred to β-Bi2O3 as source electrode and drain electrode by means of transfer electrode, and light with a wavelength of 365 nm is used as the light source to obtain a photodetector.

[0074] The photodetector prepared in Example 3 was tested for electrical and photoelectric properties using a probe station. Figure 6 . Figure 6 Schematic diagram of the structure of the photodetector prepared in Example 3 (a), IV curves under different light intensities (b), intensity-dependent responsivity and detectivity (c), EQE under different light intensities (d), IT curves under light of different wavelengths (e), and characteristic light response time curve in fast scanning mode (f). Figure 6 Part b is under 365nm light, the light power is from 0.022mW·cm -2 to 2.15 mW·cm -2 The power dependence of the photodetector was studied in the range of , and the results showed that the photocurrent increased significantly with the increase of light intensity. Figure 6 As can be seen from part c, the maximum responsivity and detectivity of the photodetector prepared in Example 3 can reach 47.44A·W -1 and 3.29×10 14 Jones. By Figure 6 As can be seen from the middle d part, its maximum EQE can reach 1.6×10 4 %.Depend on Figure 6 As can be seen from the middle e part, after multiple cycles, the photocurrent shows periodic repetition without obvious deviation, proving that the device has excellent stability and repeatability. Figure 6 As can be seen in the middle f section, the device has a rise time of 10ms and a fall time of 12ms, indicating a fast photoresponse. In summary, the above device indicators show that this photodetector performs better than most photodetectors based on two-dimensional materials.

[0075] Example 4

[0076] The two-dimensional ultra-thin non-layered material β-Bi2O3 prepared in Example 1 was made into a polarization-sensitive photodetector. The structure of the photodetector is shown in FIG. Figure 7 In a, the specific preparation process is: based on the two-dimensional ultra-thin non-layered material β-Bi2O3 synthesized in Example 1, electrodes formed by 10 nm thick Cr and 30 nm thick Au are transferred to β-Bi2O3 as source electrode and drain electrode by using a transfer electrode method, 365 nm wavelength light is used as the light source, and a half-wave plate is placed above the light source to achieve a change in the direction of the light source, thereby obtaining a polarization-sensitive photodetector.

[0077] The polarization-sensitive photodetector prepared in Example 4 was tested electrically and photoelectrically using a probe station. The direction of the laser beam was changed by rotating the half-wave plate. The results are shown in Figure 2. Figure 7 . Figure 7 Schematic diagram of the structure of the polarization-sensitive photodetector prepared in Example 4 (a), IV curve under periodic change of polarization angle (b), polar coordinate diagram of polarization-dependent photocurrent (c), and polar coordinate diagram of polarization-dependent responsivity (d). Figure 7 As can be seen from part b, when the direction of the laser beam changes periodically over time, a periodically changing photocurrent will be generated. Figure 7 Extract the data from part b of the figure and draw a polar coordinate diagram of the polarization-dependent photocurrent and responsivity, as shown in Figure 2. Figure 7 As shown in the cd part. Figure 7 The middle CD portion shows that the photocurrent and responsivity vary periodically with the rotation angle, reaching maximum values ​​at 90° and 270° and minimum values ​​at 0° and 180°. The calculated anisotropy ratio of photocurrent to responsivity is 1.91. These results demonstrate that the two-dimensional, ultrathin, non-layered β-Bi2O3 material prepared in Example 1 exhibits strong in-plane photoelectric anisotropy, providing an ideal platform for multifunctional optoelectronic devices.

[0078] The above are merely preferred embodiments of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of protection of the claims.

Claims

1. A surface passivation-assisted growth method for two-dimensional ultra-thin non-layered material β-Bi2O3, characterized in that: The following steps are involved: Using Bi2O3 as a precursor and Bi2Se3 as an auxiliary agent, a two-dimensional ultra-thin non-layered material β-Bi2O3 was obtained by vapor deposition.

2. The surface passivation assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 1, characterized in that: The mass ratio of Bi2O3 to Bi2Se3 is 2:

1.

3. The surface passivation assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 1, characterized in that: The vapor deposition includes the following steps: placing Bi2O3 and Bi2Se3 at the heat source center and upstream of a tubular furnace respectively, placing fluorophlogopite directly above Bi2O3, then heating to the growth temperature for crystal growth, and then cooling to room temperature to obtain the two-dimensional ultra-thin non-layered material β-Bi2O3.

4. The surface passivation-assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 3, characterized in that: The distance between the fluorophlogopite and Bi2O3 is 4 mm.

5. The surface passivation assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 3, characterized in that: The fluorophlogopite mica further comprises a pre-treatment step before use; the pre-treatment method is: peeling the fluorophlogopite mica and using the freshly dissociated surface as the crystal growth surface.

6. The surface passivation assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 3, characterized in that: The growth temperature is 680-750°C.

7. The surface passivation-assisted growth method of two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 3, characterized in that: The crystal growth time is 20-60 minutes.

8. A two-dimensional ultra-thin non-layered material β-Bi2O3 obtained by the surface passivation assisted growth method of the two-dimensional ultra-thin non-layered material β-Bi2O3 as described in any one of claims 1 to 7.

9. The two-dimensional ultra-thin non-layered material β-Bi2O3 according to claim 8, characterized in that: The thinnest thickness of the two-dimensional ultra-thin non-layered material β-Bi2O3 is 0.77nm, and the maximum lateral size is 163μm.

10. Application of the two-dimensional ultra-thin non-layered material β-Bi2O3 according to any one of claims 8 to 9 in the field of optoelectronics.

Citation Information

Patent Citations

  • High-mobility-ratio lamellar Bi2O2Se semiconductor film and preparation method thereof

    CN106011783A

  • Two-dimensional bismuth-oxide selenide crystal and near-infrared light based electric detector

    CN106783552A

  • Method for preparing two-dimensional non-layered wide-band-gap oxide based on Van der Waals epitaxy

    CN115287750A

  • Method of forming a p-type group II-VI semiconductor crystal layer on a substrate

    US20040058463A1

  • Nano-thin BixOySez low-temperature oxygen transporter membrane for oxygen transport, separation, and two-dimensional (2D) material manipulation

    US20230264972A1