NiO / NiFe2O4 magnetic heterogeneous nanoparticles as well as preparation method and application thereof
The sol-gel method of NiO/NiFe2O4 magnetic heterogeneous nanoparticles is synthesized by the sol-gel method, and the electron spin polarization is regulated by the built-in magnetic field, which solves the problem of limited performance of existing catalysts, and achieves efficient electrolytic oxygen precipitation reaction and stability Improved performance and suitable for engineering applications.
Patent Information
- Application Number
- CN202410407456.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-12-06
AI Technical Summary
The performance of existing catalysts in the oxygen precipitation reaction during the electrolytic process is limited, and external magnetic field regulation is complex and industrial application difficulties, making it difficult to achieve efficient electronic spin structure regulation.
NiO/NiFe2O4 magnetic heterogeneous nanoparticles were designed to synthesize NiO/NiFe2O4 through sol-gel method to form nanoparticles rich in heterointerfaces, and use the built-in magnetic field to regulate electron spin polarization to improve catalytic performance.
It realizes the excellent activity and ultrafast reaction kinetics of the catalyst, the current density is improved and the stability is significant, and the process is simple and the cost is low, making it suitable for engineering applications.
Smart Images

Figure CN119082777A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material technology and relates to a magnetic heterostructure catalyst for water electrolysis anode, in particular to a NiO / NiFe2O4 magnetic heterostructure catalyst and a preparation method and application thereof. Background Art
[0002] The increasingly severe energy and environmental problems have made the development and utilization of new clean energy (such as hydrogen energy, solar energy, etc.) urgent. On the road to realizing the implementation of hydrogen production infrastructure, the continuous optimization of the efficiency of the electrolytic water tank is crucial, among which the performance of the anode oxygen evolution reaction catalyst is the key to affecting the efficiency of the electrolytic water tank. At present, the design of catalysts is mainly based on the Sabatier theory, but the optimal catalyst expected by this theory has faced a performance bottleneck. Since the water decomposition process is related to the spin properties of electrons, it is expected to break the bottleneck and achieve another breakthrough in performance by regulating the electronic spin structure of the catalyst. At present, researchers use external magnetic fields to regulate the electronic spin structure of magnetic oxide catalysts to improve performance, breaking the limitations of the Sabatier theory.
[0003] This simple and clean method brings new hope for performance breakthroughs in magnetic transition metal oxide catalysts. Although the introduction of an external magnetic field is an effective means of improving performance, there are still some drawbacks and challenges: ① The external magnetic field applied by the magnet is limited, resulting in unsatisfactory performance improvement; ② The introduction of an external magnetic field will bring about some complex physical effects, which will make the entire catalytic system complicated and difficult to clarify the catalytic mechanism; ③ It is very difficult to implement the external magnetic field in industrial applications, and it will bring additional energy consumption. Therefore, it is of great significance to scientific research and engineering applications to design magnetic heterostructure catalysts and construct a "built-in magnetic field" at the heterogeneous interface to regulate the electron spin structure and thereby greatly improve the electrocatalytic performance. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing and applying NiO / NiFe2O4 magnetic heterogeneous nanoparticles. The NiO / NiFe2O4 catalyst prepared by the present invention is a nanoparticle rich in heterogeneous interfaces, and the particle size is 20-50nm. The heterostructure exhibits intrinsic ferromagnetism and has a controllable "built-in magnetic field" at the interface, which can reach a maximum of 2594.37Oe. The strong built-in magnetic field at the interface regulates the electron spin polarization of the catalyst and promotes the efficient generation of triplet oxygen in the process of water electrolysis. Therefore, the material exhibits excellent catalytic activity and ultrafast reaction kinetics, and the corresponding current density at 1.7V is 118.32mA cm -2 , the Tafel slope is 56.90mV / dec.
[0005] The NiO / NiFe2O4 magnetic heterogeneous nanoparticles in the present invention are synthesized by a sol-gel method. First, a mixed solution of a metal salt precursor, a swelling agent, and a condensing agent is heated to form a gel, the gel is baked at a low temperature to make it swell, and finally a heat treatment is performed to make the precursor undergo phase segregation crystallization, thereby obtaining a high-quality nickel-iron-based heterogeneous structure catalyst with a built-in magnetic field.
[0006] The method for preparing NiO / NiFe2O4 magnetic heterogeneous nanoparticles provided by the present invention comprises the following steps:
[0007] 1) dissolving nickel-based metal salt, iron-based metal salt, bulking agent and complexing agent in dilute nitric acid and stirring to form a uniform solution;
[0008] 2) continuously heating the solution obtained in step 1) to evaporate the water to form a non-fluid gel;
[0009] 3) baking the gel obtained in step 2) until the swelling agent is fully decomposed, generating a large amount of gas to expand the gel to form a black fluffy product, and then grinding the product in a mortar into a black powder.
[0010] 4) subjecting the black powder obtained in step 3) to high temperature heat treatment to cause segregation crystallization to form a heterogeneous structure catalyst.
[0011] In the above step 1), the nickel-based metal salt is preferably nickel acetate, nickel nitrate, nickel chloride, etc., and nickel acetate tetrahydrate is the most preferred; the iron-based metal salt is preferably iron nitrate, iron chloride, iron sulfate, etc., and iron nitrate nonahydrate is the most preferred; the bulking agent is preferably citric acid; and the complexing agent is preferably urea. The concentration of the dilute nitric acid is preferably 5%-20%; the concentration of the nickel-based metal salt is 0.01-0.5 mol / L; the concentration of the iron-based metal salt is preferably 0.01-0.5 mol / L; the concentration of the bulking agent is preferably 0.1-1 mol / L; and the concentration of the complexing agent is preferably 0.1-1 mol / L.
[0012] In the above step 2), the heating temperature is preferably 70-110° C., most preferably 85-95° C.; the heating time is preferably 3-8 hours, most preferably 4-5 hours.
[0013] In the above step 3), the puffing temperature is preferably 120-180° C., most preferably 150-170° C.; the puffing time is preferably 8-24 hours, most preferably 10-14 hours.
[0014] In the above step 4), the heat treatment temperature is preferably 400-1000° C., the heat treatment time is preferably 4-10 hours, and high-purity oxygen is introduced as a carrier gas during the process.
[0015] The catalyst preparation method of the invention is simple, low in cost, high in yield and has engineering application prospects.
[0016] The present invention further provides magnetic testing of the above-mentioned NiO / NiFe2O4 heterogeneous nanoparticles and electrochemical testing of NiO / NiFe2O4 heterogeneous structure catalysts. The magnetic testing of NiO / NiFe2O4 heterogeneous nanoparticles confirms that the heterogeneous structure catalyst has a strong built-in magnetic field, which realizes the fine regulation of the electron spin structure. In addition, the electrocatalytic performance test of NiO / NiFe2O4 heterogeneous nanoparticles confirms that the catalyst exhibits excellent catalytic activity and ultrafast reaction kinetics, which are better than commercial catalysts, indicating that the regulation of the electron spin structure effectively improves the performance of the catalyst. At the same time, the catalyst has excellent stability and still maintains excellent catalytic activity after 15 working days. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 In the figure, (a) is a transmission electron micrograph of the NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 1, and (b), (c), and (d) are the corresponding element distribution diagrams, respectively.
[0018] Figure 2 This is the X-ray diffraction analysis diagram of the NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 1.
[0019] Figure 3 In the figure, (a) is a high-resolution transmission electron micrograph of NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 1, and (b) and (c) are the corresponding atomic phase diagrams, respectively.
[0020] Figure 4 Magnetic hysteresis loop diagram of NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 1 under field cooling and zero-field cooling modes.
[0021] Figure 5 In the figure, (a) is a transmission electron micrograph of the NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 2, and (b), (c), and (d) are the corresponding element distribution diagrams, respectively.
[0022] Figure 6 Magnetic hysteresis loop diagram of NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 2 under field cooling and zero-field cooling modes.
[0023] Figure 7 In the figure, (a) is a transmission electron micrograph of the NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 3, and (b), (c), and (d) are the corresponding element distribution diagrams, respectively.
[0024] Figure 8The hysteresis loop diagram of NiO / NiFe2O4 heterogeneous nanoparticles prepared in Example 3 under field cooling and zero-field cooling modes.
[0025] Fig. 9 This is a graph of the electrochemical performance (linear sweep voltammetry) of Example 4 using NiO / NiFe2O4 heterogeneous nanoparticles as anode catalyst for water electrolysis.
[0026] Fig.10 This is the Tafel slope diagram of Example 4 using NiO / NiFe2O4 heterogeneous nanoparticles as anode catalyst for water electrolysis.
[0027] Fig.11 This is a stability curve diagram of Example 4 using NiO / NiFe2O4 heterogeneous nanoparticles as anode catalyst for water electrolysis. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] 1.680g of nickel acetate tetrahydrate, 0.303g of ferric nitrate nonahydrate, 2.881g of citric acid and 0.901g of urea were weighed in sequence and dissolved in 5% dilute nitric acid, and magnetically stirred for 20 minutes to obtain a transparent and uniform solution. The above solution was heated in an oil bath at a constant temperature of 85°C for 5 hours, and magnetic stirring was continued during the process until the water evaporated to form a gel. Subsequently, the gel was placed in an oven, kept at 170°C for 12 hours, and then taken out after naturally cooling to room temperature, and fully ground for 10 minutes to obtain a black powder. Finally, the black powder was spread on a clean crucible and placed in a tubular furnace. First, the gas in the furnace was replaced with oxygen three times, and then heat-treated in an oxygen atmosphere, heated to 600°C at a rate of 5°C / min and kept warm for 6 hours, and after naturally cooling to room temperature, a brown powder sample was obtained, which was NiO / NiFe2O4 heterogeneous nanoparticles.
[0031] like Figure 1 As shown in the figure, the size, morphology and element distribution of NiO / NiFe2O4 heterogeneous nanoparticles were characterized by transmission electron microscopy. From Figure (a), it can be seen that the particle size is about 30nm. From Figures (b)-(d), it can be seen that Ni and Fe elements are unevenly distributed while O element is evenly distributed, indicating that the material prepared by the above method has different phases due to the segregation of Fe.
[0032] like Figure 2 As shown, the positions of the diffraction peaks revealed by X-ray diffraction analysis match the standard cards of NiO (JCPDS 47-1049) and NiFe2O4 (JCPDS 54-0964), respectively, indicating that the material prepared by the above method has two physical phases of NiO and NiFe2O4.
[0033] like Figure 3 As shown in the figure, the interface and atomic phases in different regions of NiO / NiFe2O4 heterogeneous nanoparticles were characterized by high-resolution transmission electron microscopy. Figure (a) shows that there is a heterogeneous interface inside the particles, and it can be seen that the atomic structures on both sides of the interface are different. Figure (b) is the atomic phase of spinel structure NiFe2O4, and Figure (c) is the atomic phase of cubic structure NiO.
[0034] like Figure 4 As shown, the magnetic exchange bias curve proves the intrinsic ferromagnetism of the NiO / NiFe2O4 heterogeneous nanoparticles, with a coercive force of 1744.71Oe. From the offset of the hysteresis loop in the field cooling mode, it can be seen that the material has a strong built-in magnetic field, which can reach 2594.37Oe.
[0035] Example 2
[0036] 1.555g of nickel acetate tetrahydrate, 0.505g of ferric nitrate nonahydrate, 2.881g of citric acid and 0.901g of urea were weighed in sequence and dissolved in 5% dilute nitric acid, and magnetically stirred for 20 minutes to obtain a transparent and uniform solution. The above solution was heated in an oil bath at a constant temperature of 90°C for 4 hours, and magnetic stirring was continued during the process until the water evaporated to form a gel. Subsequently, the gel was placed in an oven, kept at 180°C for 12 hours, and then taken out after naturally cooling to room temperature, and fully ground for 10 minutes to obtain a black powder. Finally, the black powder was spread on a clean crucible and placed in a tubular furnace. First, the gas in the furnace was replaced with oxygen three times, and then heat-treated in an oxygen atmosphere, heated to 600°C at a rate of 5°C / min and kept warm for 6 hours. After naturally cooling to room temperature, a brown powder sample was obtained, which was NiO / NiFe2O4 heterogeneous nanoparticles.
[0037] like Figure 5 As shown, the size, morphology and element distribution of the NiO / NiFe2O4 heterogeneous nanoparticles were characterized by transmission electron microscopy. From Figure a), it can be seen that the particle size is about 30nm. From Figures b)-d), it can be seen that Ni and Fe elements are unevenly distributed while O element is evenly distributed, indicating that the material prepared by the above method has different phases due to the segregation of Fe.
[0038] like Figure 6As shown, the magnetic exchange bias curve proves the intrinsic ferromagnetism of the NiO / NiFe2O4 heterogeneous nanoparticles, with a coercive force of 1116.55 Oe. From the offset of the hysteresis loop in the field cooling mode, it can be seen that the material has a built-in magnetic field of 543.65 Oe.
[0039] Example 3
[0040] 1.089g of nickel acetate tetrahydrate, 1.263g of ferric nitrate nonahydrate, 2.881g of citric acid and 0.901g of urea were weighed in sequence and dissolved in 5% dilute nitric acid, and magnetically stirred for 20 minutes to obtain a transparent and uniform solution. The above solution was heated in an oil bath at a constant temperature of 95°C for 4 hours, and magnetic stirring was continued during the process until the water evaporated to form a gel. Subsequently, the gel was placed in an oven, kept at 170°C for 12 hours, and then taken out after naturally cooling to room temperature, and fully ground for 10 minutes to obtain a black powder. Finally, the black powder was spread on a clean crucible and placed in a tubular furnace. First, the gas in the furnace was replaced with oxygen three times, and then heat-treated in an oxygen atmosphere, heated to 600°C at a rate of 5°C / min and kept warm for 6 hours, and after naturally cooling to room temperature, a brown powder sample was obtained, which was NiO / NiFe2O4 heterogeneous nanoparticles.
[0041] like Figure 7 As shown, the size, morphology and element distribution of the NiO / NiFe2O4 heterogeneous nanoparticles were characterized by transmission electron microscopy. From Figure a), it can be seen that the particle size is about 30nm. From Figures b)-d), it can be seen that Ni and Fe elements are unevenly distributed while O element is evenly distributed, indicating that the material prepared by the above method has different phases due to the segregation of Fe.
[0042] like Figure 8 As shown, the magnetic exchange bias curve proves the intrinsic ferromagnetism of the NiO / NiFe2O4 heterogeneous nanoparticles, with a coercive force of 995.20Oe. From the offset of the hysteresis loop in the field cooling mode, it can be seen that the material has a built-in magnetic field of 164.12Oe.
[0043] Example 4
[0044] The NiO / NiFe2O4 heterogeneous nanomaterial prepared in Example 1 was used as an electrolytic water anode catalyst to test its electrocatalytic performance. The material was ultrasonically homogenized in isopropanol and Nafion membrane solution to prepare a viscous catalyst slurry, which was evenly coated on a glassy carbon electrode to test the electrochemical performance of the electrolytic water anode catalyst.
[0045] like Fig. 9 As shown in Figure 2, the current density of the catalyst at 1.7 V is 118.32 mA cm -2 , indicating that the catalyst has excellent catalytic activity and is superior to commercial catalysts.
[0046] like Fig.10 As shown, the Tafel slope of the catalyst is 56.90 mV / dec, indicating that the catalyst has ultrafast reaction kinetics and accelerates the efficient generation of triplet oxygen.
[0047] like Fig.11 As shown, the catalyst -2 The catalyst can run stably for 120 hours at the current density, indicating that it has excellent stability and still maintains excellent catalytic activity after 15 working days.
Claims
1. A NiO / NiFe2O4 heterogeneous nanoparticle, characterized in that: The particle size is 20-50nm, with intrinsic ferromagnetism, and there is a NiO and NiFe2O4 two-phase interface inside the particle, and there is a built-in magnetic field at the interface, which can reach a maximum of 2594.37Oe.
2. The method for preparing the NiO / NiFe2O4 heterogeneous nanoparticles according to claim 1, comprising the following steps: 1) dissolving nickel-based metal salt, iron-based metal salt, bulking agent and complexing agent in dilute nitric acid and stirring to form a uniform solution; 2) continuously heating the solution obtained in step 1) to evaporate the water therein to form a non-fluid gel; 3) placing the gel obtained in step 2) into an oven and heating it to fully decompose the swelling agent to form a black fluffy product, and then fully grinding the product to obtain a black powder; 4) subjecting the black powder obtained in step 3) to high temperature heat treatment to cause segregation and crystallization to form heterogeneous structure nanoparticles.
3. The preparation method according to claim 2, characterized in that: Step 1) The nickel-based metal salt is preferably nickel acetate, nickel nitrate, nickel chloride, etc., and is most preferably nickel acetate tetrahydrate; the concentration of the nickel-based metal salt substance is 0.01-0.5 mol / L.
4. The preparation method according to claim 2, characterized in that: In step 1), the iron-based metal salt is preferably ferric nitrate, ferric chloride, ferric sulfate, etc., and most preferably ferric nitrate nonahydrate; the concentration of the iron-based metal salt is preferably 0.01-0.5 mol / L.
5. The preparation method according to claim 2, characterized in that: In step 1), the swelling agent is preferably citric acid, and the concentration of the swelling agent is preferably 0.1-1 mol / L; the complexing agent is preferably urea, and the concentration of the complexing agent is preferably 0.1-1 mol / L; the concentration of the dilute nitric acid is preferably 5%-20%.
6. The preparation method according to claim 2, characterized in that: Step 2) The heating temperature is preferably 70-110° C., and the heating time is preferably 3-8 hours.
7. The preparation method according to claim 2, characterized in that: Step 3) The puffing temperature is preferably 120-180° C., and the puffing time is preferably 8-24 hours.
8. The preparation method according to claim 2, characterized in that: Step 4) The heat treatment temperature is preferably 400-1000° C., the heat treatment time is preferably 4-10 hours, and high-purity oxygen is introduced as a carrier gas during the process.
9. Use of the NiO / NiFe2O4 heterogeneous nanoparticles according to claim 1 as an electrocatalyst.
10. The use according to claim 7, characterized in that The electrocatalyst is an anode catalyst for electrolyzing water.