Two-component polyester fiber fabric and preparation method thereof

Through the preparation method of two-component polyester fiber fabric, the combined melt spinning technology of modified polyester particles and ordinary polyester particles is used to form 'peanut' cross-sectional fibers, which solves the problem of insufficient breathability of existing polyester fiber fabrics , significantly improves the breathability of the fabric.

CN119082903APending Publication Date: 2024-12-06HANGZHOU KELI NETWORK TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411386132.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polyester fiber fabrics have not yet functionally met the diverse needs of consumers and are not breathable.

Method used

Using the preparation method of two-component polyester fiber fabric, the modified polyester particles and ordinary polyester particles are dried at low temperature and sliced, melt-spinned to form a two-component polyester fiber with a "peanut" cross-section, and the modification is made. The bending deformation of the polyester when it is heated/wet increases the gap between the yarns and improves breathability.

Benefits of technology

It realizes the diverse functions and comprehensive performance of the fabric, significantly improves breathability, and meets the wider needs of consumers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082903A_ABST
    Figure CN119082903A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of fabrics, and particularly relates to a two-component polyester fiber fabric and a preparation method thereof. The preparation method comprises the following steps: carrying out low-temperature drying treatment on modified polyester particles, and slicing to obtain dried modified polyester chips; common polyester particles are subjected to low-temperature drying treatment and sliced, and dried common polyester slices are obtained; respectively placing the dried modified polyester chip and the dried common polyester chip in a spinning device, respectively melting, passing through respective melt pipelines, and reaching the same spinneret orifice; spinning temperature is controlled, two kinds of polyester are sprayed out to form fibers, and then the fibers are sequentially subjected to rectification cross air blowing, oiling, drafting and winding forming processes. The double-component polyester fiber fabric is diversified in function and comprehensive in performance, the peanut-shaped double-component polyester fibers obtained through melt spinning can be bent and deformed after being heated / wetted, so that gaps among the fabric yarns are enlarged, the air permeability is improved, and more diversified requirements of consumers can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fabrics, and in particular relates to a two-component polyester fiber fabric and a preparation method thereof. Background Art

[0002] Polyester fiber fabric is a synthetic fiber obtained by spinning polyester formed by the condensation of organic dibasic acids and diols. Its trade name is polyester, and it is currently the largest variety of synthetic fibers.

[0003] Polyester has many excellent textile properties and wearing properties, and is widely used. It can be spun pure or blended with other fibers. Currently, the polyester fiber fabrics on the market are still to be improved in function and cannot meet the diverse needs of consumers. Based on this, the technical solution of the present invention is proposed. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a method for preparing a two-component polyester fiber fabric, the preparation method comprising the following steps:

[0005] (1) low-temperature drying and slicing the modified polyester particles to obtain dried modified polyester slices;

[0006] (2) drying the common polyester particles at low temperature and slicing them to obtain dry common polyester slices;

[0007] (3) placing the dried modified polyester chips and the dried ordinary polyester chips in spinning devices respectively, and then melting them respectively and passing through their respective melt pipes and reaching the same spinneret hole;

[0008] (4) The spinning temperature is controlled to spray the two polyesters into fibers, and then the fibers are subjected to the processes of rectifying side blowing, oiling, drawing, and winding to obtain the two-component polyester fiber fabric.

[0009] Among them: the modified polyester particles are prepared by adding a hygroscopic / heat-expanding substance (sodium alginate) to ordinary polyester particles and then melt-granulating them. The modified polyester particles and conventional polyester particles can be melt-spun to produce "peanut"-shaped two-component polyester fibers (two polyesters are separated, half is modified polyester and the other half is conventional polyester). The "peanut"-shaped two-component polyester fibers will bend and deform when exposed to heat / humidity (only the modified polyester will twist and deform), thereby enlarging the gaps between the yarns of the fabric and increasing the air permeability.

[0010] Preferably, in step (1), the temperature of the low-temperature drying treatment is 40-45° C.; and the time of the low-temperature drying treatment is 4-5 hours.

[0011] Preferably, in step (2), the temperature of the low-temperature drying treatment is 40-45° C.; and the time of the low-temperature drying treatment is 4-5 hours.

[0012] Preferably, in step (3), the mass ratio of the dried modified polyester chips to the dried ordinary polyester chips is 1:1.

[0013] Preferably, in step (3), the melting temperature is 250-260°C.

[0014] Preferably, in step (4), the spinning temperature is: the vapor phase temperature is 275-277°C, the temperature of the first screw zone is 263-267°C, the temperature of the second screw zone is 268-272°C, the temperature of the third screw zone is 273-277°C, the temperature of the fourth screw zone is 276-280°C, and the temperature of the fifth screw zone is 277-281°C;

[0015] And / or, during the spinning process, the pressure of the spinning assembly is 10 MPa.

[0016] Preferably, in step (4), in the rectifying side blowing process, the blowing temperature is 23-25° C., the blowing humidity is 80-90%, and the blowing speed is 0.5-0.6 m / s.

[0017] Preferably, in step (4), in the oiling process, the oil agent used is Japan Takemoto F-1782, with a concentration of 11.5-12.5%.

[0018] Preferably, in step (4), in the winding forming process, the winding speed is 3700 m / min and the winding tension is 0.16 g / D.

[0019] Based on the same technical concept, the present invention further provides a two-component polyester fiber fabric obtained by the above preparation method.

[0020] The beneficial effects of the present invention are:

[0021] The two-component polyester fiber fabric of the present invention has various functions and comprehensive performances, wherein: the modified polyester and the ordinary polyester are melted separately and then pass through their respective melting pipes, and are distributed in a composite assembly composed of a plurality of distribution plates, and finally reach the spinneret and are ejected from the same spinneret hole to form fibers, thereby forming a two-component polyester fiber with a "peanut-shaped" cross-section. In the "peanut-shaped" two-component polyester fiber, the modified polyester will bend and deform when exposed to heat / humidity, thereby enlarging the gaps between the yarns of the fabric and increasing the air permeability, thereby being able to meet more diverse needs of consumers. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 The present invention is a process flow chart for preparing a two-component polyester fiber fabric. DETAILED DESCRIPTION

[0024] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0025] Example 1

[0026] This embodiment provides a method for preparing a two-component polyester fiber fabric, the preparation method comprising the following steps:

[0027] (1) transporting 500 g of modified polyester pellets to a low-temperature drying device, drying them at 40° C. for 5 h, and then slicing them to obtain dried modified polyester chips;

[0028] (2) 500 g of common polyester pellets were transported to a low-temperature drying device and dried at 40° C. for 5 h, and then sliced ​​to obtain dry common polyester chips;

[0029] (3) placing the dried modified polyester chips and the dried ordinary polyester chips in a spinning device respectively, melt-extruding at 250° C., and then melting and passing through respective melt pipes, filtering and entering a metering pump, and finally reaching a spinneret and then spinning from the same spinneret hole;

[0030] Among them, the spinning temperature is: the vapor phase temperature is 275°C, the temperature of the screw zone 1 is 263°C, the temperature of the screw zone 2 is 268°C, the temperature of the screw zone 3 is 273°C, the temperature of the screw zone 4 is 276°C, and the temperature of the screw zone 5 is 277°C;

[0031] (4) Under the condition of an assembly pressure of 10 MPa, the two polyesters are ejected from the spinneret holes to form fibers, and then sequentially undergo side blowing (blowing temperature is 23°C, blowing humidity is 80%, and blowing speed is 0.5 m / s), oiling (the oil agent is Japan Takemoto F-1782, with a concentration of 11.5%), pre-network (pre-network pressure is 0.7 kg), stretching, heat setting, main network (main network pressure is 3.4 kg), soft winding (winding speed is 3700 m / min, winding tension is 0.16 g / D), texturing, inspection, and packaging to obtain the two-component polyester fiber fabric.

[0032] Example 2

[0033] This embodiment provides a method for preparing a two-component polyester fiber fabric, the preparation method comprising the following steps:

[0034] (1) transporting 500 g of modified polyester pellets to a low-temperature drying device, drying them at 45° C. for 4 h, and then slicing them to obtain dried modified polyester chips;

[0035] (2) 500 g of common polyester pellets were transported to a low-temperature drying device and dried at 45° C. for 4 h, and then sliced ​​to obtain dry common polyester chips;

[0036] (3) placing the dried modified polyester chips and the dried ordinary polyester chips in a spinning device respectively, melt-extrude them at 260° C., and then melt them respectively and pass through their respective melt pipes, filter them and enter a metering pump, and finally reach a spinneret and then spin out from the same spinneret hole;

[0037] Among them, the spinning temperature is: the vapor phase temperature is 277°C, the temperature of the screw zone 1 is 267°C, the temperature of the screw zone 2 is 272°C, the temperature of the screw zone 3 is 277°C, the temperature of the screw zone 4 is 280°C, and the temperature of the screw zone 5 is 281°C;

[0038] (4) Under the condition of an assembly pressure of 10 MPa, the two polyesters are ejected from the spinneret holes to form fibers, and then sequentially undergo side blowing (blowing temperature is 25°C, blowing humidity is 90%, and blowing speed is 0.6 m / s), oiling (the oil agent is Japan Takemoto F-1782, with a concentration of 12.5%), pre-network (pre-network pressure is 0.9 kg), stretching, heat setting, main network (main network pressure is 3.6 kg), soft winding (winding speed is 3700 m / min, winding tension is 0.16 g / D), texturing, inspection, and packaging to obtain the two-component polyester fiber fabric.

[0039] Example 3

[0040] This embodiment provides a method for preparing a two-component polyester fiber fabric, the preparation method comprising the following steps:

[0041] (1) transporting 500 g of modified polyester pellets to a low-temperature drying device, drying them at 42° C. for 4.5 h, and then slicing them to obtain dried modified polyester chips;

[0042] (2) 500 g of ordinary polyester pellets were transported to a low-temperature drying device and dried at 42° C. for 4.5 h, and then sliced ​​to obtain dry ordinary polyester chips;

[0043] (3) placing the dried modified polyester chips and the dried ordinary polyester chips in a spinning device respectively, melt-extrude them at 255° C., and then melt them respectively and pass through their respective melt pipes, filter them and enter a metering pump, and finally reach a spinneret and then spin out from the same spinneret hole;

[0044] Among them, the spinning temperature is: the vapor phase temperature is 276°C, the temperature of the screw zone 1 is 265°C, the temperature of the screw zone 2 is 270°C, the temperature of the screw zone 3 is 275°C, the temperature of the screw zone 4 is 278°C, and the temperature of the screw zone 5 is 279°C;

[0045] (4) Under the condition of an assembly pressure of 10 MPa, the two polyesters are ejected from the spinneret holes to form fibers, and then sequentially undergo side blowing (blowing temperature is 24°C, blowing humidity is 85%, and blowing speed is 0.5 m / s), oiling (the oil agent is Japan Takemoto F-1782, with a concentration of 12.0%), pre-network (pre-network pressure is 0.8 kg), stretching, heat setting, main network (main network pressure is 3.5 kg), soft winding (winding speed is 3700 m / min, winding tension is 0.16 g / D), texturing, inspection, and packaging to obtain the two-component polyester fiber fabric.

[0046] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a two-component polyester fiber fabric, characterized in that: The preparation method comprises the following steps: (1) low-temperature drying and slicing the modified polyester particles to obtain dried modified polyester slices; (2) drying the common polyester particles at low temperature and slicing them to obtain dry common polyester slices; (3) placing the dried modified polyester chips and the dried ordinary polyester chips in spinning devices respectively, and then melting them respectively and passing through their respective melt pipes and reaching the same spinneret hole; (4) The spinning temperature is controlled to spray the two polyesters into fibers, and then the fibers are subjected to the processes of rectifying side blowing, oiling, drawing, and winding to obtain the two-component polyester fiber fabric.

2. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (1), the temperature of the low-temperature drying treatment is 40-45° C.; and the time of the low-temperature drying treatment is 4-5 hours.

3. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (2), the temperature of the low-temperature drying treatment is 40 to 45° C.; and the time of the low-temperature drying treatment is 4 to 5 hours.

4. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (3), the mass ratio of the dried modified polyester chips to the dried ordinary polyester chips is 1:

1.

5. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (3), the melting temperature is 250-260°C.

6. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (4), the spinning temperatures are: vapor phase temperature is 275-277°C, screw zone 1 temperature is 263-267°C, screw zone 2 temperature is 268-272°C, screw zone 3 temperature is 273-277°C, screw zone 4 temperature is 276-280°C, and screw zone 5 temperature is 277-281°C; And / or, during the spinning process, the pressure of the spinning assembly is 10 MPa.

7. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (4), in the blowing process on the rectifying side, the blowing temperature is 23-25° C., the blowing humidity is 80-90%, and the blowing speed is 0.5-0.6 m / s.

8. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (4), in the oiling process, the oil agent used is Japan Takemoto F-1782, with a concentration of 11.5-12.5%.

9. The method for preparing the two-component polyester fiber fabric according to claim 1, characterized in that: In step (4), in the winding forming process, the winding speed is 3700m / min and the winding tension is 0.16g / D.

10. The two-component polyester fiber fabric obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polyester elastomer / PET composite elastic fiber and preparation method thereof

    CN104831417A

  • Side-by-side composite fiber and preparation method thereof

    CN109957856A

  • Hydrophilic / hydrophobic two-component polyester fiber as well as preparation method and application thereof

    CN112725931A

  • Preparation method of bi-component hot-wet comfortable polyester composite elastic fiber

    CN115449923A

  • Method for preparing waterproof breathable fabric from regenerated polyester fibers

    CN118223296A