Cloth forming process of water-soluble fibers
Through the foaming liquid coating technology of water-soluble resin, the problem of insufficient processability and strength of carboxymethyl cellulose fiber and polyvinyl alcohol fiber composite nonwoven fabric is solved, and high-strength and excellent water-soluble nonwoven fabric is achieved. The preparation of the product is suitable for a variety of application fields and improves process safety.
Patent Information
- Application Number
- CN202311335045.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-16
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the processability and strength of the composite nonwoven fabric of carboxymethyl cellulose fiber and polyvinyl alcohol fiber are insufficient, and there are problems of safety hazards and poor water solubility effects when treated with organic solvents.
The water-soluble resin is used for coating, and the water-soluble fiber is bonded and shaped by bonding materials with a foaming degree of more than 20 times to form a high-strength, hydrophilic water-soluble nonwoven fabric.
The mechanical properties of water-soluble non-woven fabrics have been improved, with a strength of 18-24N and excellent water-soluble effect. They are suitable for embroidered base cloth, beauty and other fields, and avoid the problem of water-soluble fibers not forming in glue, which improves the problem of water-soluble fibers not being formed by water-soluble in glue. Process safety.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fibers, and in particular relates to a cloth-forming process of water-soluble fibers. Background Art
[0002] Cellulose fiber is carboxymethylated to obtain carboxymethyl cellulose (CMC) fiber, which is used in dressing, cosmetics, textile and papermaking industries while maintaining the fiber state. Polyvinyl alcohol (PVA) fiber is a water-soluble synthetic fiber made of PVA using a specific process. It can be blended with other fibers and then dissolved after textile processing to obtain textiles. Carboxymethyl cellulose fiber has good water absorption, but poor strength and does not have thermoplastic processability; polyvinyl alcohol fibers such as 0588 series fibers have poor spinnability, so the non-woven fabrics made by hot rolling process have poor strength.
[0003] In order to improve the processability and strength of non-woven fabrics made of carboxymethyl cellulose fiber or carboxymethyl cellulose fiber and polyvinyl alcohol fiber composite water-soluble fiber, the prior art uses blending with other fibers with thermoplastic processability to improve the availability of carboxymethyl cellulose fiber or carboxymethyl cellulose fiber and polyvinyl alcohol fiber composite fiber. Patent No. "CN201410180772.8" is named "A water-soluble fiber for embroidery", and the water-soluble fiber for embroidery is blended and woven by polyvinyl alcohol fiber, seaweed fiber, carboxymethyl cellulose fiber and soybean oligosaccharide fiber. The weight percentage of each component in the water-soluble fiber for embroidery is 36%-48% for the polyvinyl alcohol fiber, 24%-28% for the seaweed fiber, 17%-21% for the carboxymethyl cellulose fiber, and 11%-15% for the soybean oligosaccharide fiber. By mixing with other fibers, a fiber with a certain strength and soluble in water is obtained.
[0004] Another method to improve the strength of the above fibers is to use a glue to bond the carboxymethyl cellulose fibers or polyvinyl alcohol fibers together. For example, the carboxymethyl cellulose fibers or polyvinyl alcohol fibers are bonded with acrylic glue in ethyl acetate. The prepared non-woven fabric has good strength but no hydrophilicity, poor water solubility, and a long dissolution time.
[0005] Organic solvents such as ethyl acetate are particularly flammable, especially after being immersed in glue containing organic solvents, they must be dried through a heated air duct. The heated air duct will inevitably cause static electricity and sparks, making the processing very dangerous.
[0006] The non-woven fabrics made by bonding water-soluble fibers with glues made of water-soluble resins, such as CMC glue and PVA glue, have good strength, excellent hydrophilic effect, and are non-flammable. Their applications are not limited to embroidery base fabrics, water-soluble lace, and beauty products (facial mask base materials, wipes, etc.). However, the water-soluble resin must first be prepared as an aqueous solution. If it is directly applied to the water-soluble fiber, the water-soluble fiber will not be water-soluble and will be difficult to operate. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a water-soluble fiber cloth-forming process, which realizes the purpose of using water-soluble resin to bond water-soluble fibers to prepare non-woven fabrics with high strength and excellent hydrophilic effect. The water-soluble resin aqueous solution composite surfactant is foamed and coated, the water-soluble fibers are infiltrated and dried, the fibers are bonded together by resin curing, and after shaping treatment, the water-soluble non-woven fabric is made.
[0008] After research, it was found that carboxymethyl cellulose fiber and polyvinyl alcohol fiber have different molecular structures. Polyvinyl alcohol is a linear polyhydroxy polymer with a structure of 1,3 ethylene glycol or 1,2 ethylene glycol. The macromolecule is connected by a carbon-carbon chain. Its molecular chain contains a large number of hydroxyl groups, which is mainly affected by the degree of alcoholysis. Carboxymethyl cellulose is a cellulose ether obtained by alkalization and etherification of cellulose. It has a structure of unbranched straight-chain glucan composed of β-1,4-glycosidic bonds. According to the different number of hydrogen substitutions on the three hydroxyl groups of the glucose unit, carboxymethyl cellulose with different numbers of substitutions is formed. Therefore, although carboxymethyl cellulose and polyvinyl alcohol are both water-soluble polymers, the water-soluble process first undergoes swelling and then dissolution. However, due to the different molecular structures, the swelling degree is significantly different, which is manifested in that less water is required for the swelling phenomenon of polyvinyl alcohol, and more water is required for the swelling phenomenon of carboxymethyl cellulose. Generally speaking, it is relatively easy to prepare a 20% PVA aqueous solution; however, it is almost impossible to dissolve 20% carboxymethyl cellulose in 80% water because the swelling of carboxymethyl cellulose has not reached its limit and cannot be converted from swelling to dissolution.
[0009] The inventor actually utilized the characteristic of carboxymethyl cellulose with a wide swelling-dissolution range. By adding a small amount of water, the carboxymethyl cellulose fibers were bonded to each other or to glue and then dried in an oven, under the condition that the carboxymethyl cellulose fibers had not yet dissolved and the fibers could maintain a certain tensile strength. The purpose of making cloth was achieved by bonding the swollen fibers to each other or to glue and drying them in an oven.
[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0011] A water-soluble fiber cloth-forming process comprises the following steps:
[0012] S1. Foaming
[0013] The adhesive material is pumped into the foaming machine to be foamed until the foaming degree is greater than 20 times the foaming liquid.
[0014] Preferably, the density of the foaming liquid is 0.1 g / cm 3 ~0.4g / cm 3 ; The foaming degree is the liquid density before foaming (ρ 0 ) and the density of the foam after foaming (ρ 1 ) ratio.
[0015] Preferably, the bonding material comprises a water-soluble resin, distilled water, a surfactant and a plasticizer; the water-soluble resin is one or both of carboxymethyl cellulose resin and polyvinyl alcohol resin, the degree of substitution of the carboxymethyl cellulose resin is consistent with the degree of substitution of carboxymethyl cellulose fiber, and the degree of alcoholysis of the polyvinyl alcohol resin is consistent with the degree of alcoholysis of the polyvinyl alcohol fiber.
[0016] Furthermore, in the adhesive material, carboxymethyl cellulose resin accounts for 0-2% of the adhesive material mass, polyvinyl alcohol resin accounts for 0-10% of the adhesive material mass, surfactant accounts for 0.001%-3% of the adhesive material mass, plasticizer accounts for 0.2%-3% of the adhesive material mass, and the rest is distilled water.
[0017] Preferably, the surfactant is one or more of stearic acid, oleic acid, lauric acid, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium hexadecyl sulfate, sodium octadecyl sulfate, sucrose fatty acid ester, sorbitan fatty acid ester, polysorbate, benzalkonium chloride, benzalkonium bromide, lecithin, etc.
[0018] Preferably, the plasticizer is one or more of glycerol, propylene glycol, and polyethylene glycol.
[0019] Preferably, the preparation method of the adhesive material is: adding a water-soluble resin to distilled water and stirring for 5 min-10 min to obtain an aqueous solution of the water-soluble resin, and then adding a surfactant and a plasticizer and stirring for 1 min-2 min to obtain the adhesive material, and the stirring rate is 400 r / min-500 r / min.
[0020] S2, coating
[0021] The water-soluble fiber is combed and then uniformly transported forward to the first pressing roller to be pressed into a fiber web. The foaming liquid is connected between the first pressing roller and the second pressing roller through a pipeline to coat the fiber web. The coated fiber web is then fed into the second pressing roller to obtain a fiber sheet.
[0022] Preferably, the water-soluble fiber is carboxymethyl cellulose fiber or a mixture of carboxymethyl cellulose fiber and polyvinyl alcohol fiber; in the water-soluble fiber, the mass proportion of carboxymethyl cellulose fiber is 35%-100%, and the mass proportion of polyvinyl alcohol fiber is 0-65%.
[0023] Furthermore, the degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose fiber is 0.8-1.0, and the degree of alcoholysis of polyvinyl alcohol in the polyvinyl alcohol fiber is 80%-100%.
[0024] Preferably, the pressing roller consists of two round rollers, an upper roller and a lower roller.
[0025] Preferably, the uniform forward transmission rate is 5m / min-20m / min; the foaming liquid output is 0.8L / min-2.5L / min.
[0026] S3. Drying
[0027] The fiber sheets are sent to a drying tunnel for drying to form a primary cloth.
[0028] Preferably, the drying temperature is 120°C-150°C.
[0029] S4. Finalization
[0030] The initially formed fabric is shaped by a shaping roller to obtain a water-soluble nonwoven fabric.
[0031] Preferably, the shaping temperature is 120°C-160°C, and the pressure is 0.5MPa-1.2MPa.
[0032] Preferably, the weight of the water-soluble nonwoven fabric is 5 g / m 2 -30g / m 2 .
[0033] Due to the adoption of the above technical solution, the technical effects achieved by the present invention are:
[0034] 1. The water-soluble non-woven fabric prepared by the present invention has good mechanical properties, meets the process requirements, has a strength of 18-24N, and has good water solubility. It is suitable for embroidery base fabrics, water-soluble lace, beauty and cosmetics (facial mask cloth substrates, wipes, etc.) and other fields.
[0035] 2. When water-soluble resin glue is directly used to bond water-soluble fibers, due to the water solubility of the fibers, they cannot be dissolved in the glue and are difficult to operate. Therefore, the aqueous solution of the water-soluble resin is foamed with a composite surfactant to a foaming degree greater than 20 times, and then applied to the water-soluble fibers. The water-soluble fibers are wetted but not dissolved, avoiding affecting the morphology of the water-soluble fibers.
[0036] 3. After the water-soluble fiber is pressed into a fiber web, the foaming liquid is connected to the first pressing roller and the second pressing roller through a pipeline to coat the fiber web. The coated fiber web is then fed into the second pressing roller to obtain a fiber sheet, so that the foaming liquid fully infiltrates the inside of the fiber. After drying, the water-soluble resin solidifies and bonds the fibers together. After shaping, a water-soluble non-woven fabric is obtained.
[0037] 4. Adding an appropriate amount of plasticizer to the bonding material can further improve the mechanical properties of the non-woven fabric. DETAILED DESCRIPTION
[0038] The present invention is further described below in conjunction with specific embodiments.
[0039] Embodiment 1 A process for forming a water-soluble fiber cloth comprises the following steps:
[0040] S1. Foaming
[0041] The adhesive material is pumped into the foaming machine to be foamed until the foaming degree reaches 30 times the foaming liquid.
[0042] The density of the foaming liquid is 0.29 g / cm 3 ; The foaming degree is the liquid density before foaming (ρ 0 ) and the density of the foam after foaming (ρ 1 ) ratio.
[0043] The bonding material comprises a water-soluble resin, distilled water, a surfactant and a plasticizer; the water-soluble resin is a carboxymethyl cellulose resin.
[0044] In the adhesive material, carboxymethyl cellulose resin accounts for 1% of the mass of the adhesive material, surfactant accounts for 0.002% of the mass of the adhesive material, plasticizer accounts for 1.5% of the mass of the adhesive material, and distilled water accounts for 97.498% of the mass of the adhesive material.
[0045] The surfactant is sodium lauryl sulfate, and the plasticizer is glycerol.
[0046] The degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose resin is 0.9.
[0047] The preparation method of the bonding material is: adding a water-soluble resin into distilled water and stirring for 8 minutes to obtain an aqueous solution of the water-soluble resin, then adding a surfactant and a plasticizer and stirring for 1 minute to obtain the bonding material, and the stirring rate is 400 r / min.
[0048] S2, coating
[0049] The water-soluble fiber is combed and then uniformly transported forward to the first pressing roller to be pressed into a fiber web. The foaming liquid is connected between the first pressing roller and the second pressing roller through a pipeline to coat the fiber web. The coated fiber web is then fed into the second pressing roller to obtain a fiber sheet.
[0050] The water-soluble fibers are carboxymethyl cellulose fibers and polyvinyl alcohol fibers; among the water-soluble fibers, the mass proportion of the carboxymethyl cellulose fibers is 50%, and the mass proportion of the polyvinyl alcohol fibers is 50%.
[0051] The degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose fiber is 0.9, and the degree of alcoholysis of polyvinyl alcohol in the polyvinyl alcohol fiber is 88%.
[0052] The pressure roller is composed of two round rollers, an upper roller and a lower roller; the uniform forward transmission rate is 10 m / min; and the foaming liquid output is 1.2 L / min.
[0053] S3. Drying
[0054] The fiber sheets are sent to a drying tunnel for drying to form a primary cloth.
[0055] The drying temperature is 140°C.
[0056] S4. Finalization
[0057] The initially formed fabric is shaped by a shaping roller to obtain a water-soluble nonwoven fabric.
[0058] The setting temperature is 150° C. and the pressure is 1 MPa.
[0059] The weight of the water-soluble nonwoven fabric is 20 g / m 2 .
[0060] Embodiment 2 A process for forming a water-soluble fiber cloth comprises the following steps:
[0061] S1. Foaming
[0062] The adhesive material is pumped into the foaming machine to be foamed until the foaming degree reaches 40 times the foaming liquid.
[0063] The density of the foaming liquid is 0.2 g / cm 3 ; The foaming degree is the liquid density before foaming (ρ 0 ) and the density of the foam after foaming (ρ 1 ) ratio.
[0064] The bonding material comprises a water-soluble resin, distilled water, a surfactant and a plasticizer; the water-soluble resin is a polyvinyl alcohol resin.
[0065] In the adhesive material, the polyvinyl alcohol resin accounts for 10% of the mass of the adhesive material, the surfactant accounts for 0.001% of the mass of the adhesive material, the plasticizer accounts for 0.2% of the mass of the adhesive material, and the rest is distilled water.
[0066] The surfactant is sodium dodecylbenzene sulfonate, and the plasticizer is propylene glycol.
[0067] The alcoholysis degree of the polyvinyl alcohol in the polyvinyl alcohol resin is 85%.
[0068] The preparation method of the bonding material is: adding a water-soluble resin into distilled water and stirring for 5 minutes to obtain an aqueous solution of the water-soluble resin, then adding a surfactant and a plasticizer and stirring for 1 minute to obtain the bonding material, and the stirring rate is 400 r / min.
[0069] S2, coating
[0070] The water-soluble fiber is combed and then uniformly transported forward to the first pressing roller to be pressed into a fiber web. The foaming liquid is connected between the first pressing roller and the second pressing roller through a pipeline to coat the fiber web. The coated fiber web is then fed into the second pressing roller to obtain a fiber sheet.
[0071] The water-soluble fiber is carboxymethyl cellulose fiber; the degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose fiber is 0.9.
[0072] The pressure roller is composed of two round rollers, an upper roller and a lower roller; the uniform forward transmission rate is 5 m / min; and the foaming liquid output is 0.8 L / min.
[0073] S3. Drying
[0074] The fiber sheets are sent to a drying tunnel for drying to form a primary cloth.
[0075] The drying temperature is 120°C.
[0076] S4. Finalization
[0077] The initially formed fabric is shaped by a shaping roller to obtain a water-soluble nonwoven fabric.
[0078] The setting temperature is 160° C. and the pressure is 1.2 MPa.
[0079] The weight of the water-soluble nonwoven fabric is 5g / m 2 .
[0080] Embodiment 3 A process for forming a water-soluble fiber cloth comprises the following steps:
[0081] S1. Foaming
[0082] The adhesive material is pumped into the foaming machine to be foamed until the foaming degree reaches 20.2 times to form a foaming liquid.
[0083] The density of the foaming liquid is 0.4 g / cm 3 ; The foaming degree is the liquid density before foaming (ρ 0 ) and the density of the foam after foaming (ρ1 ) ratio.
[0084] The bonding material comprises a water-soluble resin, distilled water, a surfactant and a plasticizer; the water-soluble resin is carboxymethyl cellulose resin and polyvinyl alcohol resin.
[0085] In the adhesive material, carboxymethyl cellulose resin accounts for 2% of the adhesive material mass, polyvinyl alcohol resin accounts for 3% of the adhesive material mass, surfactant accounts for 3% of the adhesive material mass, plasticizer accounts for 3% of the adhesive material mass, and the rest is distilled water.
[0086] The surfactant is sodium lauryl sulfate, and the plasticizer is glycerol.
[0087] The degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose resin is 0.9, and the degree of alcoholysis of polyvinyl alcohol in the polyvinyl alcohol resin is 85%.
[0088] The preparation method of the bonding material is: adding a water-soluble resin into distilled water and stirring for 10 minutes to obtain an aqueous solution of the water-soluble resin, then adding a surfactant and a plasticizer and stirring for 2 minutes to obtain the bonding material, and the stirring rate is 500 r / min.
[0089] S2, coating
[0090] The water-soluble fiber is combed and then uniformly transported forward to the first pressing roller to be pressed into a fiber web. The foaming liquid is connected between the first pressing roller and the second pressing roller through a pipeline to coat the fiber web. The coated fiber web is then fed into the second pressing roller to obtain a fiber sheet.
[0091] The water-soluble fibers are carboxymethyl cellulose fibers and polyvinyl alcohol fibers; among the water-soluble fibers, the mass proportion of the carboxymethyl cellulose fibers is 35%, and the mass proportion of the polyvinyl alcohol fibers is 65%.
[0092] The degree of substitution of carboxymethyl cellulose in the carboxymethyl cellulose fiber is 0.9, and the degree of alcoholysis of polyvinyl alcohol in the polyvinyl alcohol fiber is 85%.
[0093] The pressure roller is composed of two round rollers, an upper roller and a lower roller; the uniform forward transmission rate is 20 m / min; and the foaming liquid output is 2.5 L / min.
[0094] S3. Drying
[0095] The fiber sheets are sent to a drying tunnel for drying to form a primary cloth.
[0096] The drying temperature is 150°C.
[0097] S4. Finalization
[0098] The initially formed fabric is shaped by a shaping roller to obtain a water-soluble nonwoven fabric.
[0099] The setting temperature is 120° C. and the pressure is 0.5 MPa.
[0100] The weight of the water-soluble nonwoven fabric is 30 g / m 2 .
[0101] The various properties of the water-soluble non-woven fabrics prepared by the methods of Examples 1-3 were tested, wherein the test standard for the strength of the non-woven fabrics is GB / T 3923.1-2013, as shown in Table 1.
[0102] Table 1
[0103] Example Example 1 Example 2 Example 3 strength 22N 18N 24N Water dissolution temperature ≥20℃ ≥0℃ ≥20℃ Water dissolution time 3min 1min 5min
[0104] It can be seen that the water-soluble non-woven fabrics prepared by the methods of Examples 1-3 have good strength, excellent water-soluble effect and stronger applicability.
[0105] Unless otherwise specified, the ratios and percentages described in the present invention are all weight ratios and weight percentages; and the raw materials are all commercially available.
[0106] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for forming a cloth of water-soluble fiber, It is characterized in that The process includes foaming, coating, drying and shaping.
2. A process for forming a water-soluble fiber according to claim 1, It is characterized in that The foaming comprises pumping the adhesive material into a foaming machine to foam the adhesive material until the foaming degree is greater than 20 times the foaming liquid; The density of the foaming liquid is 0.1 g / cm 3 ~0.4g / cm 3 .
3. A process for forming a water-soluble fiber according to claim 2, It is characterized in that The bonding material comprises a water-soluble resin, distilled water, a surfactant and a plasticizer; the water-soluble resin is one or both of carboxymethyl cellulose resin and polyvinyl alcohol resin.
4. A process for forming a water-soluble fiber cloth according to claim 3, It is characterized in that In the adhesive material, carboxymethyl cellulose resin accounts for 0-2% of the adhesive material mass, polyvinyl alcohol resin accounts for 0-10% of the adhesive material mass, surfactant accounts for 0.001%-3% of the adhesive material mass, plasticizer accounts for 0.2%-3% of the adhesive material mass, and the rest is distilled water.
5. A process for forming a water-soluble fiber cloth according to claim 3, It is characterized in that The surfactant is one or more of stearic acid, oleic acid, lauric acid, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium hexadecyl sulfate, sodium octadecyl sulfate, sucrose fatty acid ester, sorbitan fatty acid ester, polysorbate, benzalkonium chloride, benzalkonium bromide, lecithin, etc.; Preferably, the plasticizer is one or more of glycerol, propylene glycol, and polyethylene glycol.
6. A process for forming a water-soluble fiber cloth according to claim 3, It is characterized in that The preparation method of the bonding material is: adding a water-soluble resin into distilled water and stirring for 5-10 minutes to obtain an aqueous solution of the water-soluble resin, then adding a surfactant and a plasticizer and stirring for 1-2 minutes to obtain the bonding material, and the stirring rate is 400r / min-500r / min.
7. A process for forming a water-soluble fiber cloth according to claim 1, It is characterized in that The coating comprises the following steps: the water-soluble fiber is combed and then uniformly conveyed forward to be fed into a first pressing roller to be pressed into a fiber web; a foaming liquid is introduced into the space between the first pressing roller and the second pressing roller through a pipeline to coat the fiber web; and the coated fiber web is then fed into a second pressing roller to obtain a fiber sheet; The water-soluble fiber is carboxymethyl cellulose fiber or a mixture of carboxymethyl cellulose fiber and polyvinyl alcohol fiber; in the water-soluble fiber, the mass proportion of the carboxymethyl cellulose fiber is 35%-100%, and the mass proportion of the polyvinyl alcohol fiber is 0-65%.
8. A process for forming a water-soluble fiber cloth according to claim 7, It is characterized in that The uniform forward transmission rate is 5m / min-20m / min; the foaming liquid output is 0.8L / min-2.5L / min.
9. A process for forming a water-soluble fiber cloth according to claim 1, It is characterized in that The drying process involves sending the fiber sheets into a drying tunnel for drying to form a primary fabric; The drying temperature is 120°C-150°C.
10. A process for forming a water-soluble fiber cloth according to claim 1, It is characterized in that The shaping is to shape the initial fabric through a shaping roller to obtain a water-soluble nonwoven fabric; The setting temperature is 120°C-160°C and the pressure is 0.5MPa-1.2MPa; The weight of the water-soluble nonwoven fabric is 5g / m 2 -30g / m 2 .
Citation Information
Patent Citations
Ground fabric for embroidery and process for producing the same
CN101522976A
Production method of polyvinyl alcohol fiber composite modified material for machine-made products
CN110820340A
Non-woven water-soluble wipe
CN114040744A
Synthetic cloth, method and system for the production of said cloth
CN1871391A
Water-absorbing nonwoven fabric sheet and method for producing the same
JP2007197862A