Magnetorheological fluid composite material with negative Poisson's ratio characteristic and preparation method thereof
By combining negative Poisson's ratio fabric with magnetorheological fluid, the fabric structure and surface modification treatment improves shear and settlement resistance, solving the problems of easy settlement and poor sealing of magnetorheological fluid materials, achieving different Excellent performance and low sealing requirements under operating conditions.
Patent Information
- Application Number
- CN202411192352.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Magnetorheological liquid materials are easy to settle and difficult to seal in practical applications, and the shear resistance and controllable yield stress requirements are difficult to meet.
Using a composite material of negative Poisson's ratio fabric and magnetorheological fluid, the composite material is formed by immersing the negative Poisson's ratio fabric in magnetorheological fluid, and the concave hexagonal array mesh structure and surface modification treatment of the fabric Improve shear resistance and settlement resistance, and improve the adsorption capacity of the material through the modification and distribution of magnetic particles.
The magnetorheological liquid composite material has strong shear resistance, good settlement resistance, stable working performance, and low sealing requirements, which can adapt to excellent magnetorheological effects under different working conditions.
Smart Images

Figure CN119083185A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to smart materials, and in particular to a magnetorheological fluid composite material with negative Poisson's tropy characteristics and a preparation method thereof. Background Art
[0002] Smart materials are new functional materials that can adjust their own characteristics by sensing changes in external stimuli and responding quickly, thereby being able to adapt to environmental changes. Magnetorheological fluid, as an important branch of smart materials, can quickly change from liquid and solid-like states in milliseconds according to changes in external magnetic field stimuli, producing a magnetorheological effect. At present, due to the huge density difference between the continuous phase and the dispersed phase of magnetorheological fluid materials, its sedimentation stability and reliability have been difficult to meet the needs of practical applications. Many researchers have explored how to improve the anti-sedimentation ability of magnetorheological fluids, but most of them are by optimizing the performance of the liquid continuous phase or seeking a better material formula; at the same time, for some special working conditions, the yield stress requirements of the material are getting higher and higher.
[0003] Therefore, it is necessary to meet the requirements of excellent magnetorheological effect, anti-settling performance, and controllable yield stress of magnetorheological fluid under different working conditions, and solve the problems of easy sedimentation and difficult sealing of magnetorheological materials in practical applications. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a magnetorheological fluid composite material with negative Poisson's ratio characteristics and a preparation method thereof. The composite of magnetorheological fluid and negative Poisson's ratio material can meet the requirements of excellent magnetorheological effect, anti-settling performance, and controllable yield stress under different working conditions, and solve the problems of easy sedimentation and difficult sealing of magnetorheological materials in practical applications.
[0005] The magnetorheological fluid composite material with negative Poisson's ratio characteristics of the present invention is composited by magnetorheological fluid and negative Poisson's ratio material;
[0006] Further, the negative Poisson's ratio material is a negative Poisson's ratio fabric, and the magnetorheological fluid material is attached to the negative Poisson's ratio fabric;
[0007] Further, the magnetorheological fluid composite material is formed by dipping a negative Poisson's ratio fabric into a magnetorheological fluid;
[0008] Furthermore, the Poisson's ratio fabric is woven from elastic yarns and non-elastic yarns into a special concave hexagonal array grid;
[0009] Furthermore, the Poisson's ratio fabric is subjected to surface modification treatment to enhance the fabric's oil absorption;
[0010] Furthermore, the surface modification treatment of the Poisson's ratio fabric comprises the following steps: soaking the Poisson's ratio fabric in a stearic acid solution, performing ultrasonic dispersion, vacuum drying, and then repeatedly washing with anhydrous ethanol and repeatedly drying;
[0011] Furthermore, the magnetorheological fluid raw materials include, by weight: 1 part of base fluid, 0.15-0.35 parts of modified magnetic particles, 0.002-0.02 parts of thickener, and 0.005-0.025 parts of surfactant;
[0012] Furthermore, the base liquid is dimethyl silicone oil or mineral oil, the thickener is fumed silica, and the surfactant is one or a mixture of two or more of oleic acid, stearic acid, and glycerol;
[0013] Furthermore, the preparation method of the modified magnetic particles comprises the following steps:
[0014] a. Cleaning of magnetic particles;
[0015] b. Mix the silane coupling agent, hexadecyltrimethylsilane and isopropanol solution, then add the cleaned magnetic particles for ultrasonic dispersion, ball mill and then dry to obtain modified magnetic particles.
[0016] The method for preparing the magnetorheological fluid composite material having negative Poisson's tropy property of the present invention comprises the following steps:
[0017] The negative Poisson's ratio fabric is fully immersed in the magnetorheological fluid and ultrasonically dispersed so that each yarn has obvious magnetorheological fluid adhesion, and then vacuum dried.
[0018] The beneficial effects of the present invention are as follows: the magnetorheological fluid composite material with negative Poisson's ratio characteristics and the preparation method thereof, the magnetorheological fluid composite material prepared by compounding the magnetorheological fluid with the negative Poisson's ratio material has the characteristics of strong shear resistance, good anti-sedimentation performance, stable working performance, and low sealing requirements for the use occasions. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0020] Figure 1 Schematic diagram of the concave hexagonal structure of negative Poisson's ratio fabric;
[0021] Figure 2 is the deformation behavior of negative Poisson's ratio fabric (when negative Poisson's ratio fabric is stretched vertically, the fabric will expand along the horizontal (weft) direction, thereby producing a negative Poisson's ratio effect in the vertical direction). DETAILED DESCRIPTION
[0022] The magnetorheological fluid composite material with negative Poisson's ratio characteristics of this embodiment is composed of a magnetorheological fluid and a negative Poisson's ratio material, the negative Poisson's ratio material is a negative Poisson's ratio fabric, and the magnetorheological fluid material is attached to the negative Poisson's ratio fabric; the negative Poisson's ratio material can expand laterally when stretched, and shrink laterally when compressed, showing a "tensile expansion effect". Therefore, the negative Poisson's ratio material has good shear modulus, impact resistance and energy absorption performance, which also makes the negative Poisson's ratio material have certain applications in the field of vibration and impact. However, the ability of pure negative Poisson's ratio fabric to resist broadband vibration and impact is still insufficient. Therefore, combined with the unique rheological properties of the magnetorheological fluid material, the composite material can have reversible and controllable energy absorption characteristics, which better solves the vibration problem. At the same time, since conventional magnetorheological fluids face the problem of easy sedimentation, which will cause the performance of the material to fail, the support and adsorption of the spatial fibers inside the negative Poisson's ratio fabric can effectively improve the anti-sedimentation performance of the magnetorheological material. When a negative Poisson's ratio fabric is stretched vertically, the fabric will expand along the horizontal (weft) direction, resulting in a negative Poisson's ratio effect in the vertical direction, such as Figure 2 As shown. The magnetorheological fluid material itself has good controllable anti-shear performance, and the prepared negative Poisson's ratio material has good anti-shear performance. The magnetorheological fluid and the spatial fibers inside the negative Poisson's ratio fabric "complement each other", and the magnetic particles are attached between the fibers, and the viscosity of the base fluid itself makes the magnetic particles better distributed in the base fluid, and the "anti-lodging" ability of the fabric fibers is also effectively improved, so the anti-shear performance is enhanced; the spatial fibers of the negative Poisson's ratio fabric can effectively solve the sedimentation problem of the magnetorheological fluid material, and the fibers can support the attached magnetic particles to a certain extent, thereby improving the anti-sedimentation performance of the magnetorheological fluid material; because the spatial fibers of the negative Poisson's ratio fabric can better absorb the magnetorheological fluid, in actual use, it is only necessary to place the composite material in the working gap, and there is no need to fill the working chamber like conventional magnetorheological fluid, so the use requirements for sealing are relatively low; for high-frequency shear conditions, the viscosity of the magnetorheological fluid itself and the dispersion of the magnetic particles can enhance the friction between the fabric fibers, prevent the slippage of the fabric fibers, and effectively broaden the energy absorption frequency band of the material in the medium and high frequency micro-amplitude excitation conditions.
[0023] In this embodiment, the magnetorheological fluid composite material is formed by impregnating a negative Poisson's ratio fabric in a magnetorheological fluid; the raw material of the fabric can be selected from cotton, aramid, polyester, nylon and other materials according to the specific use conditions and the weaving conditions of the fabric.
[0024] In this embodiment, the Poisson's ratio fabric is woven into a special concave hexagonal array grid by elastic yarn and inelastic yarn; polyvinyl alcohol is used to size the yarn surface to increase the strength of the yarn and facilitate weaving; and it is woven by using elastic and inelastic yarns using a rapier loom and a multi-arm opening device.
[0025] According to the application scenario characteristics of the vibration isolation device, negative Poisson's ratio fabrics with different minimum unit structures are selected. Figure 1 As shown in FIG. 1 , the minimum repeating fabric structural unit of the negative Poisson's ratio fabric is a concave polygon, which is mainly composed of warp yarns and weft yarns interwoven together, so that the woven fabric exhibits negative Poisson's ratio characteristics in the horizontal and vertical directions of its plane (the vertical direction has the best effect). Figure 1 As shown in the figure, the green lines are elastic yarns, and the rest are inelastic yarns. This avoids interference between warp yarns of different lengths when the fabric is stretched, and the fabric can have a certain shape recovery ability. Figure 1 The "double Y-shaped" structure of the concave hexagons connected inside the grid shown can prevent the structure from being too loose when the fabric is stretched, provide appropriate restraining force, and enhance the material's shear resistance.
[0026] In this embodiment, the Poisson's ratio fabric is subjected to surface modification to enhance the fabric's oil absorption; the surface modification of the Poisson's ratio fabric includes the following steps: soaking the Poisson's ratio fabric in a stearic acid solution, performing ultrasonic dispersion, vacuum drying, and then repeatedly washing with anhydrous ethanol and repeatedly drying; the mass ratio of stearic acid is set between 1-5%. Depending on the specific working conditions, the Poisson's ratio fabric can be used in a single layer or multiple layers.
[0027] In this embodiment, the magnetorheological fluid raw materials include, by weight: 1 part of base liquid, 0.15-0.35 parts of modified magnetic particles, 0.002-0.02 parts of thickener, and 0.005-0.025 parts of surfactant; the above ratios are based on the mass fraction of the base liquid. The base liquid is dimethyl silicone oil or mineral oil, the thickener is fumed silica, and the surfactant is one or a mixture of two or more of oleic acid, stearic acid, and glycerol; the magnetic particles can be selected from conventional hydroxy iron powder or iron oxide materials, and the preparation method of the modified magnetic particles includes the following steps:
[0028] a. Cleaning of magnetic particles: The surface of the magnetic particles was cleaned by immersing them in an isopropanol solution, stirring for 15 min, then ultrasonically dispersing for 30 min, and finally drying them in a vacuum drying oven at 60 ° C or less to obtain clean magnetic particles;
[0029] b. Mix the silane coupling agent, hexadecyltrimethylsilane and isopropanol solution, then add the cleaned magnetic particles for ultrasonic dispersion, ball mill and then dry to obtain modified magnetic particles.
[0030] The preparation method of the magnetorheological fluid composite material with negative Poisson's tropy property of this embodiment comprises the following steps:
[0031] The negative Poisson's ratio fabric is fully immersed in the magnetorheological fluid and ultrasonically dispersed so that each yarn has obvious magnetorheological fluid adhesion, and then vacuum dried.
[0032] Embodiment 1
[0033] The magnetorheological fluid composite material with negative Poisson's tropy characteristic of this embodiment comprises, in parts by weight, 1 part of base fluid, 0.25 parts of modified magnetic particles, 0.01 parts of thickener, and 0.02 parts of surfactant; the base fluid is dimethyl silicone oil, the thickener is fumed silica, the surfactant is oleic acid, and the magnetic particles are hydroxy iron powder.
[0034] 1. Surface modification of negative Poisson's ratio fabric: soak the fabric in stearic acid solution and perform ultrasonic dispersion for 30 minutes, then place it in a vacuum drying oven and heat it at about 45°C for 1 hour, then repeatedly wash it with anhydrous ethanol, and repeatedly dry it to obtain a modified negative Poisson's ratio fabric;
[0035] 2. Preparation of magnetorheological fluid materials: 1) First, clean the surface of the magnetic particles, immerse them in an isopropanol solution, stir for 15 minutes, and then perform ultrasonic dispersion for 30 minutes. Finally, dry them in a vacuum drying oven below 60°C to obtain cleaned magnetic particles; then add 1% by mass of silane coupling agent and hexadecyltrimethylsilane to the isopropanol solution, stir evenly, add the treated magnetic particles, and perform ultrasonic dispersion. Then put the dispersed solution into a ball mill and mill it for 10 hours, and finally dry it in a vacuum drying oven below 60°C to obtain modified magnetic particles;
[0036] 2) The thickener, surfactant and base liquid are mixed, and then the modified magnetic particles are added and stirred thoroughly, and then ball milled in a ball mill.
[0037] 3. Preparation of magnetorheological fluid composite material: The modified negative Poisson's ratio fabric (single or multiple layers can be used according to specific working conditions) is fully mixed with the prepared magnetorheological fluid, and ultrasonic dispersion is used to make the negative Poisson's ratio fabric fully infiltrated with magnetorheological fluid, and each yarn has obvious magnetorheological fluid attached. Then the prepared material sample is placed in a vacuum drying oven and heated at about 45°C for 30 minutes to obtain a magnetorheological fluid composite material with negative Poisson's ratio characteristics.
[0038] Embodiment 2
[0039] The magnetorheological fluid composite material with negative Poisson's tropy characteristic of this embodiment comprises, in parts by weight, 1 part of base fluid, 0.3 parts of modified magnetic particles, 0.002 parts of thickener, and 0.015 parts of surfactant; the base fluid is mineral oil, the thickener is fumed silica, the surfactant is stearic acid, and the magnetic particles are iron oxide.
[0040] 1. Surface modification of negative Poisson's ratio fabric: soak the fabric in stearic acid solution for ultrasonic dispersion for 33 minutes, then place it in a vacuum drying oven and heat it at about 48°C for 1.1 hours, then repeatedly wash it with anhydrous ethanol, and repeatedly dry it to obtain a modified negative Poisson's ratio fabric;
[0041] 2. Preparation of magnetorheological fluid materials: 1) First, clean the surface of the magnetic particles, immerse them in an isopropanol solution, stir for 17 minutes, and then perform ultrasonic dispersion for 33 minutes. Finally, place them in a vacuum drying oven and dry them below 64°C to obtain cleaned magnetic particles; then add 1% by mass of silane coupling agent and hexadecyltrimethylsilane to the isopropanol solution, stir evenly, add the treated magnetic particles, and perform ultrasonic dispersion. Then place the dispersed solution in a ball mill and ball mill for 11 hours, and finally place it in a vacuum drying oven and dry it below 65°C to obtain modified magnetic particles;
[0042] 2) The thickener, surfactant and base liquid are mixed, and then the modified magnetic particles are added and stirred thoroughly, and then ball milled in a ball mill.
[0043] 3. Preparation of magnetorheological fluid composite material: The modified negative Poisson's ratio fabric (single or multiple layers can be used according to specific working conditions) is fully mixed with the prepared magnetorheological fluid, and ultrasonic dispersion is used to make the negative Poisson's ratio fabric fully infiltrated with magnetorheological fluid, and each yarn has obvious magnetorheological fluid attached. Then the prepared material sample is placed in a vacuum drying oven and heated at about 47°C for 28 minutes to obtain a magnetorheological fluid composite material with negative Poisson's ratio characteristics.
[0044] Embodiment 3
[0045] The magnetorheological fluid composite material with negative Poisson's tropy characteristic of this embodiment comprises, in parts by weight, 1 part of base fluid, 0.27 parts of modified magnetic particles, 0.02 parts of thickener, and 0.025 parts of surfactant; the base fluid is dimethyl silicone oil, the thickener is fumed silica, the surfactant is propylene glycol, and the magnetic particles are hydroxy iron powder and iron oxide.
[0046] 1. Surface modification of negative Poisson's ratio fabric: soak the fabric in stearic acid solution for ultrasonic dispersion for 28 minutes, then heat it in a vacuum drying oven at about 40°C for 1.5 hours, then repeatedly wash it with anhydrous ethanol, and repeatedly dry it to obtain a modified negative Poisson's ratio fabric;
[0047] 2. Preparation of magnetorheological fluid materials: 1) First, clean the surface of the magnetic particles, immerse them in an isopropanol solution, stir for 16 minutes, and then perform ultrasonic dispersion for 33 minutes. Finally, dry them in a vacuum drying oven below 58°C to obtain cleaned magnetic particles; then add 1% by mass of silane coupling agent and hexadecyltrimethylsilane to the isopropanol solution, stir evenly, add the treated magnetic particles, and perform ultrasonic dispersion. Then put the dispersed solution into a ball mill for 9.5 hours, and finally dry it in a vacuum drying oven below 55°C to obtain modified magnetic particles;
[0048] 2) The thickener, surfactant and base liquid are mixed, and then the modified magnetic particles are added and stirred thoroughly, and then ball milled in a ball mill.
[0049] 3. Preparation of magnetorheological fluid composite material: The modified negative Poisson's ratio fabric (single or multiple layers can be used according to specific working conditions) is fully mixed with the prepared magnetorheological fluid, and ultrasonic dispersion is used to make the negative Poisson's ratio fabric fully infiltrated with magnetorheological fluid, and each yarn has obvious magnetorheological fluid attached. Then the prepared material sample is placed in a vacuum drying oven and heated at about 40°C for 35 minutes to obtain a magnetorheological fluid composite material with negative Poisson's ratio characteristics.
[0050] Embodiment 4
[0051] The magnetorheological fluid composite material with negative Poisson's tropy characteristic of this embodiment comprises, in parts by weight, 1 part of base fluid, 0.15 parts of modified magnetic particles, 0.018 parts of thickener, and 0.005 parts of surfactant; the base fluid is dimethyl silicone oil and mineral oil, the thickener is fumed silica, the surfactant is oleic acid, and the magnetic particles are hydroxy iron powder.
[0052] 1. Surface modification of negative Poisson's ratio fabric: soak the fabric in stearic acid solution for ultrasonic dispersion for 30 minutes, then place it in a vacuum drying oven and heat it at about 38°C for 1.5 hours, then repeatedly wash it with anhydrous ethanol, and repeatedly dry it to obtain a modified negative Poisson's ratio fabric;
[0053] 2. Preparation of magnetorheological fluid materials: 1) First, clean the surface of the magnetic particles, immerse them in an isopropanol solution, stir for 20 minutes, and then perform ultrasonic dispersion for 40 minutes, and finally dry them in a vacuum drying oven below 70°C to obtain cleaned magnetic particles; then add 1% by mass of silane coupling agent and hexadecyltrimethylsilane to the isopropanol solution, stir evenly, add the treated magnetic particles, and perform ultrasonic dispersion. Then put the dispersed solution into a ball mill and mill for 9 hours, and finally dry it in a vacuum drying oven below 55°C to obtain modified magnetic particles;
[0054] 2) The thickener, surfactant and base liquid are mixed, and then the modified magnetic particles are added and stirred thoroughly, and then ball milled in a ball mill.
[0055] 3. Preparation of magnetorheological fluid composite material: The modified negative Poisson's ratio fabric (single or multiple layers can be used according to specific working conditions) is fully mixed with the prepared magnetorheological fluid, and ultrasonic dispersion is used to make the negative Poisson's ratio fabric fully infiltrated with magnetorheological fluid, and each yarn has obvious magnetorheological fluid attached. Then the prepared material sample is placed in a vacuum drying oven and heated at about 50°C for 25 minutes to obtain a magnetorheological fluid composite material with negative Poisson's ratio characteristics.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A magnetorheological fluid composite material having a negative Poisson's ration, characterized in that: The magnetorheological fluid composite material is composited from magnetorheological fluid and negative Poisson's ratio material.
2. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 1, characterized in that: The negative Poisson's ratio material is a negative Poisson's ratio fabric, and the magnetorheological fluid material is attached to the negative Poisson's ratio fabric.
3. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 2, characterized in that: The magnetorheological fluid composite material is formed by dipping negative Poisson's ratio fabric into magnetorheological fluid.
4. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 3, characterized in that: The Poisson's ratio fabric is woven from elastic yarns and non-elastic yarns into a special concave hexagonal array grid.
5. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 4, characterized in that: The Poisson's ratio fabric is subjected to surface modification treatment to enhance the oil absorption of the fabric.
6. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 5, characterized in that: The surface modification treatment of the Poisson's ratio fabric comprises the following steps: soaking the Poisson's ratio fabric in a stearic acid solution, performing ultrasonic dispersion, vacuum drying, and then repeatedly washing with anhydrous ethanol and repeatedly drying.
7. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 1, characterized in that: The magnetorheological fluid raw materials include, by weight: 1 part of base fluid, 0.15-0.35 parts of modified magnetic particles, 0.002-0.02 parts of thickener, and 0.005-0.025 parts of surfactant.
8. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 7, characterized in that: The base liquid is dimethyl silicone oil or mineral oil, the thickener is fumed silica, and the surfactant is one or a mixture of two or more of oleic acid, stearic acid, and glycerol.
9. The magnetorheological fluid composite material with negative Poisson's ratio characteristic according to claim 7, characterized in that: The preparation method of the modified magnetic particles comprises the following steps: a. Cleaning of magnetic particles; b. Mix the silane coupling agent, hexadecyltrimethylsilane and isopropanol solution, then add the cleaned magnetic particles for ultrasonic dispersion, ball mill and then dry to obtain modified magnetic particles.
10. The method for preparing the magnetorheological fluid composite material with negative Poisson's ratio property according to claim 2, characterized in that: The following steps are involved: The negative Poisson's ratio fabric is fully immersed in the magnetorheological fluid and ultrasonically dispersed so that each yarn has obvious magnetorheological fluid adhesion, and then vacuum dried.