Corrosion-resistant and wear-resistant microfiber cloth and preparation method thereof

By forming a modified polyurethane coating on the microfiber cloth, using fluorosilicone solution and specific additives to improve its chemical corrosion resistance and wear resistance, the problem of poor alkali corrosion resistance of the water-based polyurethane preparation microfiber cloth is solved, and the more High comprehensive performance.

CN119083194APending Publication Date: 2024-12-06DONGGUAN YINGSHENG FIBER PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410998788.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ultra-fiber cloth prepared from water-based polyurethane has poor alkali corrosion resistance, high temperature resistance and chemical resistance, which affects its application performance.

Method used

Using modified water-based polyurethane impregnation solution, the modified form is formed by immersion and solidification on the island-type non-woven base fabric by double-sided impregnation and solidification, and fluorosilicone solution and specific proportions of diisocyanate, polyester polyol, polyether polyol and other additives. Polyurethane coating improves its chemical corrosion resistance and wear resistance.

Benefits of technology

It significantly improves the chemical corrosion resistance and wear resistance of the microfiber cloth, while maintaining softness and mechanical strength, and its comprehensive performance is close to that of the microfiber cloth prepared by solvent-based polyurethane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083194A_ABST
    Figure CN119083194A_ABST
Patent Text Reader

Abstract

The invention discloses corrosion-resistant and wear-resistant microfiber cloth and a preparation method thereof, and relates to the technical field of artificial leather cloth. Corrosion-resistant and wear-resistant microfiber cloth is composed of sea-island type non-woven base cloth and a modified polyurethane coating, and the modified polyurethane coating is formed in the mode that modified waterborne polyurethane immersion liquid is subjected to double-face immersion and solidified on the sea-island type non-woven base cloth. The modified waterborne polyurethane immersion liquid is prepared from 100 to 120 parts of diisocyanate, 120 to 180 parts of poly (butylene adipate) glycol, 90 to 120 parts of polytetrahydrofuran glycol, 10 to 20 parts of trihydroxymethane, 12 to 24 parts of sodium dihydroxysulfonate, 8 to 12 parts of dimethylolpropionic acid, 12 to 18 parts of triethylamine, 200 to 300 parts of polypropylene glycol, 40 to 65 parts of fluorosilicone solution and 4.5 to 6 parts of light stabilizer. The sea-island non-woven base cloth is impregnated with the modified waterborne polyurethane immersion liquid prepared from the fluorine-silicon-containing solution, so that the softness and wear resistance of the microfiber cloth are improved, and the chemical corrosion resistance of the microfiber cloth is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of artificial leather cloth, in particular to a corrosion-resistant and wear-resistant microfiber cloth and a preparation method thereof. Background Art

[0002] Microfiber cloth is a high-tech simulated leather product. Generally, microfiber cloth is a composite material composed of island-type microfiber and polyurethane resin. It has the characteristics of structural simulation, breathability, softness, etc. It is one of the ideal substitutes for genuine leather and is widely used in sofas, automobiles, luggage, shoemaking and other fields.

[0003] At present, most of the microfiber cloths in China are prepared by toluene reduction process. The typical preparation steps are to first immerse the island-type non-woven fabric in N, N-dimethylformamide solution (DMF) of polyurethane, and then add water to make DMF and water miscible. The polyurethane will solidify on the surface of the island-type non-woven fabric to form a porous polyurethane layer, and then dissolve part of the polymer by hot toluene, extract the sea phase in the fiber, and finally obtain the microfiber cloth by drying, oiling, dyeing and other treatment processes. The microfiber cloth can be further processed by veneer or grinding to form microfiber synthetic leather. The advantage of this process of using solvent-based polyurethane impregnation is that the polyurethane layer on the surface of the microfiber cloth has a large number of microporous structures, and the microfiber synthetic leather formed by further processing is plump, soft, and has a strong leather feel. However, due to the use of a large amount of DMF as a solvent when impregnating polyurethane, the entire production process not only has a strong odor, but also causes certain pollution to the environment, and also consumes a lot of energy in the subsequent recycling and treatment of waste liquid.

[0004] As people's environmental awareness gradually increases, more and more manufacturers use water-based polyurethane systems with water instead of DMF as the dispersion medium to prepare microfiber cloth. Although the microfiber cloth made by water-based polyurethane impregnation has many advantages such as environmental protection, low VOC, and non-flammability, it still has many problems such as poor high temperature resistance, poor alkali resistance, easy hydrolysis, easy yellowing, and chemical resistance is not as good as solvent-based polyurethane impregnation. Summary of the invention

[0005] In order to improve the alkali corrosion resistance of the microfiber cloth made of water-based polyurethane while maintaining the high wear resistance and mechanical strength of the microfiber cloth, the present application provides a corrosion-resistant and wear-resistant microfiber cloth and a preparation method thereof.

[0006] In the first aspect, the present application provides a corrosion-resistant and wear-resistant microfiber cloth adopts the following technical solution: A corrosion-resistant and wear-resistant microfiber cloth, comprising an island-in-sea type non-woven base cloth and a modified polyurethane coating, wherein the modified polyurethane coating is formed by double-sided impregnation and solidification of a modified waterborne polyurethane immersion liquid on the island-in-sea type non-woven base cloth, and the modified waterborne polyurethane immersion liquid comprises the following raw materials: Diisocyanate: 100-120 parts; Polybutylene adipate diol: 120-180 parts; Polytetrahydrofuran diol: 90-120 parts; Trihydroxymethane: 10-20 parts; Sodium dihydroxysulfonate: 12-24 parts; Dimethylolpropionic acid: 8-12 parts; Triethylamine: 12-18 parts; Polypropylene glycol: 200-300 parts; 40-60 parts of fluorine silicon solution; Light stabilizer: 4.5-6 parts; Wherein, the diisocyanate comprises at least one of toluene diisocyanate, hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, the molecular weight of the polybutylene adipate diol is 1000-2000, and the molecular weight of the polytetrahydrofuran diol is 2000-3000.

[0007] By adopting the above technical scheme, a modified water-based polyurethane impregnation liquid is prepared by combining a fluorine-silicon solution with specific diisocyanates, polyester polyols, polyether polyols, chain extenders and other additives, and mixing them in a specific proportion. When the modified water-based polyurethane impregnation liquid is cured, the fluorine-silicon chain segments can be connected to the polyurethane chain segments by cross-linking and grafting. Therefore, the formed modified polyurethane coating not only has the excellent properties of water-based polyurethane, but also has the performance of some fluorine-silicon chain segments, which is not only beneficial to improving the softness and wear resistance of the microfiber cloth, but also beneficial to improving the chemical corrosion resistance of the microfiber cloth.

[0008] Optionally, the fluorine silicon solution is prepared by mixing the following raw materials in parts by weight: Vinyl-terminated fluorosilicone oil: 100 parts; Hydrogen fluorinated silicone oil: 3.2-4.8 parts; Platinum catalyst: 0.48-0.64 parts; Compatibilizer: 4.5-8 parts.

[0009] By adopting the above technical scheme, the vinyl-terminated fluorosilicone oil can undergo a cross-linking reaction with the polyurethane at a certain temperature under the initiation and catalysis of the hydrogen-containing fluorosilicone oil and the platinum catalyst, and insert the fluorosilicone rubber segment into the water-based polyurethane segment, which is beneficial to improve the mechanical strength, wear resistance and corrosion resistance of the polyurethane immersion liquid after curing, thereby improving the comprehensive performance of the microfiber cloth.

[0010] Optionally, the mass fraction of vinyl groups in the vinyl-terminated fluorosilicone oil is 1.2%-1.5%, and the mass fraction of active hydrogen in the hydrogen-containing fluorosilicone oil is 0.4%-0.6%.

[0011] By adopting the above technical scheme, when the vinyl mass fraction of the terminal vinyl fluorosilicone oil is 1.2%-1.5% and the active hydrogen mass fraction in the hydrogen-containing fluorosilicone oil is in the range of 0.4%-0.6%, the cross-linking degree of the prepared fluorosilicone solution after curing is more appropriate, and the formed modified polyurethane coating has good softness, hardness and strength, and better comprehensive performance, which is not only beneficial to improve the wear resistance of the microfiber cloth, but also can maintain the softness of the microfiber cloth, and prevent the softness of the microfiber cloth from being seriously reduced due to the excessive hardness of the modified polyurethane coating.

[0012] Optionally, the compatibilizer is prepared by mixing KH550 silane coupling agent and KH560 silane coupling agent in a weight ratio of 1:(0.8-1.2).

[0013] By adopting the above technical scheme, when the compatibilizer is a mixture of KH550 silane coupling agent and KH560 silane coupling agent, and the mixing ratio is 1:(0.8-1.2), the fluorosilicone solution can have good compatibility with both polyurethane and water, which is beneficial to promote the full mixing reaction of the fluorosilicone solution with polyurethane in the aqueous polyurethane system, and improve the reaction grafting rate of the fluorosilicone solution, thereby improving the wear resistance and chemical resistance of the modified polyurethane coating, and improving the comprehensive performance of the microfiber cloth.

[0014] Optionally, the diisocyanate is a composite mixture of the hydrogenated diphenylmethane diisocyanate and the isophorone diisocyanate, and the mixing weight ratio of the hydrogenated diphenylmethane diisocyanate to the isophorone diisocyanate is 1:(1.5-2.5).

[0015] By adopting the above technical scheme, when the diisocyanate is a compound mixture of hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, and the mixing weight ratio is 1:(1.5-2.5), the modified polyurethane coating formed by curing has a more appropriate crystallinity, which is beneficial to make the microfiber cloth have good softness and wear resistance, and its overall performance is better.

[0016] Optionally, the weight ratio of the polybutylene adipate diol to the polytetrahydrofuran diol is 1:(0.8-1).

[0017] By adopting the above technical scheme, when the weight ratio of polybutylene adipate diol to polytetrahydrofuran diol in the modified aqueous polyurethane immersion liquid is 1:(0.8-1), the obtained microfiber cloth not only has high softness, but also has good wear resistance, and the comprehensive performance of the microfiber cloth is higher.

[0018] Optionally, the weight ratio of the trihydroxymethane to the sodium dihydroxysulfonate is 1:(1-1.5).

[0019] By adopting the above technical scheme, when the weight ratio of trihydroxymethane to sodium dihydroxysulfonate is 1:(1-1.5), the prepared polyurethane has good hydrophilicity, which is beneficial to improving the dispersibility of polyurethane in water, further improving the dispersion degree of the modified waterborne polyurethane immersion liquid, and reducing the occurrence of macromolecular agglomeration.

[0020] Optionally, the light stabilizer is a mixture of UV-770 and UV-P in a weight ratio of 1:(0.5-0.6).

[0021] By adopting the above technical scheme, when the light stabilizers in the modified waterborne polyurethane immersion solution are selected to be UV-770 and UV-P and are mixed with each other in a weight ratio of 1: (0.5-0.6), a certain synergistic effect can be produced between UV-770 and UV-770, and the modified polyurethane coating has better light stability and weather resistance, which is beneficial to improving the comprehensive performance of the microfiber cloth made of waterborne polyurethane.

[0022] Optionally, the method for preparing the modified aqueous polyurethane immersion liquid comprises the following steps: A1. First, polybutylene adipate diol, polytetrahydrofuran diol, trihydroxymethane and sodium dihydroxysulfonate are placed in a vacuum dehydration environment at 110-120° C., then fully stirred and mixed, cooled to 58-62° C. and added with diisocyanate, stirred evenly and then slowly heated to 65-76° C. and continued to react for 1-2 hours, then polypropylene glycol was added and continued to react for 1-2 hours to obtain a polyurethane prepolymer; A2. Cool the polyurethane prepolymer obtained in step A1 to 50-55° C., then add dimethylolpropionic acid, triethylamine, fluorine silicon solution and light stabilizer while stirring, and keep stirring the reaction for 2-3 hours. Finally, use deionized water for high-speed dispersion and emulsification to obtain a modified waterborne polyurethane immersion liquid.

[0023] By adopting the above technical scheme, the fluorosilicone solution is beneficial to fully react with the polyurethane prepolymer while undergoing the curing and cross-linking reaction, and the grafting rate of the fluorosilicone chain segment on the polyurethane is increased, which is beneficial to improve the wear resistance of the modified polyurethane coating and improve the comprehensive performance of the microfiber cloth.

[0024] In the second aspect, the present application provides a method for preparing a corrosion-resistant and wear-resistant microfiber cloth using the following technical solution: A corrosion-resistant and wear-resistant microfiber cloth and a preparation method thereof, comprising the following steps: S1. Immerse the island-in-sea type nonwoven fabric in a modified waterborne polyurethane immersion solution, control the liquid content to 85%-100%, then scrape off excess modified waterborne polyurethane immersion solution on the surface, and place the island-in-sea type nonwoven fabric at 100-120° C. for drying and solidification to obtain an impregnated fabric; S2. Put the impregnated base fabric obtained in step S1 into toluene for weight reduction, continue soaking for 2-3 hours, and finally dry the impregnated base fabric after weight reduction to obtain a corrosion-resistant and wear-resistant microfiber fabric.

[0025] By adopting the above technical solution, when the sea island type non-woven base fabric is impregnated, when the liquid content is controlled at 85%-100%, the modified aqueous polyurethane impregnation liquid can fully penetrate into the sea island type non-woven base fabric, which is conducive to uniformly forming a modified polyurethane coating on both sides and inside of the sea island type non-woven base fabric, thereby facilitating the preparation of a microfiber fabric with uniform performance. Secondly, the preparation method is simple and convenient, which is conducive to subsequent mass production.

[0026] In summary, the technical solution of this application has at least one of the following beneficial effects: 1. Impregnating the island-type non-woven fabric with a modified aqueous polyurethane impregnation solution made of fluorine-silicon solution is beneficial not only to improving the softness and wear resistance of the microfiber fabric, but also to improving the chemical corrosion resistance of the microfiber fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the structural cross-section of a corrosion-resistant and wear-resistant microfiber cloth disclosed in Example 1 of the present application.

[0028] Description of reference numerals: 1. Sea-island type non-woven fabric; 2. Modified polyurethane coating. DETAILED DESCRIPTION

[0029] The present application is further described in detail below in conjunction with the accompanying drawings, preparation examples, embodiments and comparative examples.

[0030] Preparation Example [Preparation Example 1-1] A fluorine silicon solution is prepared by mixing the following raw materials in parts by weight: 100g vinyl-terminated fluorosilicone oil, 3.2g hydrogen-containing fluorosilicone oil, 0.64g platinum catalyst and 4.5g compatibilizer.

[0031] In this preparation example, the vinyl mass fraction of the vinyl-terminated fluorosilicone oil is 1.5%; the hydrogen-containing fluorosilicone oil is grade NFS7402, and the active hydrogen mass fraction of this grade of hydrogen-containing fluorosilicone oil is 0.4%; the platinum catalyst is chloroplatinic acid; the compatibilizer is a mixture of KH550 silane coupling agent and KH560 silane coupling agent in a weight ratio of 1:0.8, that is, the addition amount of KH550 silane coupling agent is 2.5g, and the addition amount of KH560 silane coupling agent is 2g.

[0032] [Preparation Example 1-2] A fluorine silicon solution is prepared by mixing the following raw materials in parts by weight: 100g vinyl-terminated fluorosilicone oil, 4.8g hydrogen-containing fluorosilicone oil, 0.48g platinum catalyst and 8g compatibilizer.

[0033] In this preparation example, the vinyl mass fraction of the vinyl-terminated fluorosilicone oil is 1.2%; the hydrogen-containing fluorosilicone oil is grade NFS7403, and the active hydrogen mass fraction of this grade of hydrogen-containing fluorosilicone oil is 0.6%; the platinum catalyst is chloroplatinic acid; the compatibilizer is prepared by mixing KH550 silane coupling agent and KH560 silane coupling agent in a weight ratio of 1:1.2, that is, the added amount of KH550 silane coupling agent is 3.64g, and the added amount of KH560 silane coupling agent is 4.36g.

[0034] [Preparation Example 1-3] A fluorosilicone solution, which differs from [Preparation Example 1-1] in that it contains different hydrogen fluorosilicone oil.

[0035] In this preparation example, the hydrogen-containing fluorosilicone oil is NFS7403, and the active hydrogen mass fraction of this grade of hydrogen-containing fluorosilicone oil is 0.6%. [Preparation Example 1-4] A fluorosilicone solution, which differs from [Preparation Example 1-1] in that it contains different hydrogen fluorosilicone oil.

[0036] In this preparation example, the hydrogen-containing fluorosilicone oil is NFS7404, and the active hydrogen mass fraction of this grade of hydrogen-containing fluorosilicone oil is 0.8%. [Preparation Example 2-1] A modified waterborne polyurethane impregnation liquid comprises the following raw materials: 100g of diisocyanate, 150g of polybutylene adipate diol, 100g of polytetramethylene glycol diol, 15g of trihydroxymethane, 15g of sodium dihydroxysulfonate, 10g of dimethylolpropionic acid, 16g of triethylamine, 200g of polypropylene glycol, 50g of fluorosilicone solution and 4.5g of light stabilizer.

[0037] In this preparation example, hydrogenated diphenylmethane diisocyanate is selected as diisocyanate; polybutylene adipate diol is selected from polybutylene adipate diol with a molecular weight of 1000; polytetrahydrofuran diol is selected from polytetrahydrofuran diol with a molecular weight of 2000; the fluorosilicone solution is selected from the fluorosilicone solution prepared in [Preparation Example 1-1]; the molecular weight of polypropylene glycol is 200, specifically PPG-200 is selected; the light stabilizer is a mixture of UV-770 and UV-P in a weight ratio of 1:0.5, that is, the addition amount of UV-770 is 3g, and the addition amount of UV-P is 1.5.

[0038] A method for preparing a modified waterborne polyurethane immersion liquid comprises the following steps: A1. First, polybutylene adipate diol, polytetrahydrofuran diol, trihydroxymethane and sodium dihydroxysulfonate are placed in a 120° C. environment for vacuum dehydration, then stirred and mixed, cooled to 58° C. and added with diisocyanate, stirred evenly and then slowly heated to 65° C. and continued to react for 2 h, then polypropylene glycol was added and continued to react for 2 h to obtain a polyurethane prepolymer; A2. Cool the polyurethane prepolymer obtained in step A1 to 50° C., then add dimethylolpropionic acid, triethylamine, fluorosilicone solution and light stabilizer while stirring, and keep stirring the reaction for 3 hours. Finally, use deionized water for high-speed dispersion and emulsification to obtain a modified waterborne polyurethane immersion liquid.

[0039] [Preparation Example 2-2] A modified waterborne polyurethane impregnation liquid comprises the following raw materials: 120g of diisocyanate, 120g of polybutylene adipate diol, 120g of polytetramethylene glycol diol, 10g of trihydroxymethane, 24g of sodium dihydroxysulfonate, 12g of dihydroxymethylpropionic acid, 12g of triethylamine, 250g of polypropylene glycol, 40g of fluorosilicone solution, and 6g of light stabilizer.

[0040] In this preparation example, toluene diisocyanate is selected as diisocyanate; polybutylene adipate diol is selected from polybutylene adipate diol with a molecular weight of 2000; polytetrahydrofuran diol is selected from polytetrahydrofuran diol with a molecular weight of 2000; the fluorosilicone solution is selected from the fluorosilicone solution prepared in [Preparation Example 1-2]; the molecular weight of polypropylene glycol is 200, specifically PPG-200 is selected; the light stabilizer is a mixture of UV-770 and UV-P in a weight ratio of 1:0.6, that is, the addition amount of UV-770 is 3.75g, and the addition amount of UV-P is 2.25g.

[0041] A method for preparing a modified waterborne polyurethane immersion liquid comprises the following steps: A1. First, polybutylene adipate diol, polytetrahydrofuran diol, trihydroxymethane and sodium dihydroxysulfonate are placed in a 120° C. environment for vacuum dehydration, then fully stirred and mixed, cooled to 62° C. and diisocyanate is added, stirred evenly and then slowly heated to 76° C. for continuous reaction for 1 hour, polypropylene glycol is added and the reaction is continued for 1 hour to obtain a polyurethane prepolymer; A2. Cool the polyurethane prepolymer obtained in step A1 to 55° C., then add dimethylolpropionic acid, triethylamine, fluorosilicone solution and light stabilizer while stirring, and keep stirring the reaction for 2 hours. Finally, use deionized water for high-speed dispersion and emulsification to obtain a modified waterborne polyurethane immersion solution.

[0042] [Preparation Example 2-3] A modified waterborne polyurethane impregnation liquid comprises the following raw materials: 110g of diisocyanate, 180g of polybutylene adipate diol, 90g of polytetramethylene glycol, 20g of trihydroxymethane, 12g of sodium dihydroxysulfonate, 8g of dihydroxymethylpropionic acid, 16g of triethylamine, 300g of polypropylene glycol, 65g of fluorosilicone solution, and 6g of light stabilizer.

[0043] In this preparation example, the diisocyanate is a mixture of hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, and the mixing weight ratio of hydrogenated diphenylmethane diisocyanate to isophorone diisocyanate is 1:1.5, that is, the addition amount of hydrogenated diphenylmethane diisocyanate is 44g, and the addition amount of isophorone diisocyanate is 66g; polybutylene adipate diol is polybutylene adipate diol with a molecular weight of 2000; polytetrahydrofuran diol is polytetrahydrofuran diol with a molecular weight of 3000; the fluorosilicone solution is the fluorosilicone solution prepared in [Preparation Example 1-2]; the molecular weight of polypropylene glycol is 200, and specifically PPG-200 is selected; the light stabilizer is UV-770 and UV-P mixed according to a weight ratio of 1:0.6, that is, the addition amount of UV-770 is 4g, and the addition amount of UV-P is 2g.

[0044] A method for preparing a modified waterborne polyurethane immersion liquid comprises the following steps: A1. First, polybutylene adipate diol, polytetrahydrofuran diol, trihydroxymethane and sodium dihydroxysulfonate are placed in a 110°C environment for vacuum dehydration, then fully stirred and mixed, cooled to 60°C and diisocyanate is added, stirred evenly and then slowly heated to 68°C for continuous reaction for 2h, polypropylene glycol is added and the reaction is continued for 2h to obtain a polyurethane prepolymer; A2. Cool the polyurethane prepolymer obtained in step A1 to 55° C., then add dimethylolpropionic acid, triethylamine, fluorosilicone solution and light stabilizer while stirring, and keep stirring the reaction for 2 hours. Finally, use deionized water for high-speed dispersion and emulsification to obtain a modified waterborne polyurethane immersion solution.

[0045] [Preparation Example 2-4] A modified waterborne polyurethane impregnation liquid, which differs from [Preparation Example 2-1] in that the diisocyanate is different.

[0046] In this preparation example, the diisocyanate is isophorone diisocyanate.

[0047] [Preparation Example 2-5] A modified waterborne polyurethane impregnation liquid, which differs from [Preparation Example 2-1] in that the diisocyanate is different.

[0048] In this preparation example, the diisocyanate is a mixture of hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, and the mixing weight ratio of hydrogenated diphenylmethane diisocyanate to isophorone diisocyanate is 1:1.5, that is, the addition amount of hydrogenated diphenylmethane diisocyanate is 40g, and the addition amount of isophorone diisocyanate is 60g.

[0049] [Preparation Example 2-6] A modified waterborne polyurethane impregnation liquid, which differs from [Preparation Example 2-1] in that the diisocyanate is different.

[0050] In this preparation example, the diisocyanate is a mixture of hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, and the mixing weight ratio of hydrogenated diphenylmethane diisocyanate to isophorone diisocyanate is 1:2.5, that is, the addition amount of hydrogenated diphenylmethane diisocyanate is 28.57g, and the addition amount of isophorone diisocyanate is 71.43g.

[0051] [Preparation Example 2-7] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-6] in that the added amounts of polybutylene adipate diol and polytetrahydrofuran diol are different.

[0052] In this preparation example, the total addition amount of polybutylene adipate diol and polytetrahydrofuran diol is 250g, and the weight ratio between polybutylene adipate diol and polytetrahydrofuran diol is 1:0.8, i.e. the addition amount of polybutylene adipate diol is 138.9g, and the addition amount of tetrahydrofuran diol is 111.1g.

[0053] [Preparation Example 2-8] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-6] in that the added amounts of polybutylene adipate diol and polytetrahydrofuran diol are different.

[0054] In this preparation example, the total addition amount of polybutylene adipate diol and polytetrahydrofuran diol is 250g, and the weight ratio between polybutylene adipate diol and polytetrahydrofuran diol is 1:1, that is, the addition amount of polybutylene adipate diol is 125g, and the addition amount of tetrahydrofuran diol is 125g.

[0055] [Preparation Example 2-9] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-8] in that the added amounts of trihydroxymethane and sodium dihydroxysulfonate are different.

[0056] In this preparation example, the total amount of trihydroxymethane and sodium dihydroxysulfonate added is 30g, and the weight ratio between hydroxymethane and sodium dihydroxysulfonate is 1:1.5, that is, the amount of polybutylene adipate diol added is 12g, and the amount of tetrahydrofuran diol added is 18g.

[0057] [Preparation Example 2-10] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-9] in that the fluorine-silicon solution is different.

[0058] In this preparation example, the fluorine silicon solution is a fluorine silicon solution prepared in [Preparation Example 1-3].

[0059] [Preparation Example 2-11] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-9] in that the fluorine-silicon solution is different.

[0060] In this preparation example, the fluorine silicon solution is a fluorine silicon solution prepared in [Preparation Example 1-4].

[0061] [Preparation Example 2-12] A modified waterborne polyurethane immersion liquid, which differs from [Preparation Example 2-1] in that no fluorine-silicon solution is added. Example

[0062] [Example 1] A corrosion-resistant and wear-resistant microfiber cloth, such as Figure 1 As shown, it is composed of an island-in-sea type non-woven fabric 1 and a modified polyurethane coating 2, wherein the modified polyurethane coating 2 is formed by double-sided impregnation and coagulation of a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-1] on the island-in-sea type non-woven fabric 1.

[0063] A method for preparing a corrosion-resistant and wear-resistant microfiber cloth comprises the following steps: S1. Immerse the island-in-sea nonwoven fabric 1 in a modified aqueous polyurethane immersion solution, control the liquid content to 95%, then scrape off the excess modified aqueous polyurethane immersion solution on the surface, and place the island-in-sea nonwoven fabric 1 at 120°C for drying and solidification to obtain an impregnated fabric; S2. Put the impregnated fabric obtained in step S1 into toluene for reduction, continue to soak for 2 hours, and finally dry the reduced impregnated fabric to obtain a corrosion-resistant and wear-resistant microfiber cloth.

[0064] [Example 2] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating and the preparation method are different.

[0065] In this embodiment, the modified polyurethane coating 2 is formed by double-sided impregnation and solidification of a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-2] on the island-in-sea non-woven fabric 1.

[0066] A method for preparing a corrosion-resistant and wear-resistant microfiber cloth comprises the following steps: S1. Immerse the island-in-sea nonwoven fabric 1 in a modified aqueous polyurethane immersion liquid, control the liquid content to 85%, then scrape off the excess modified aqueous polyurethane immersion liquid on the surface, and place the island-in-sea nonwoven fabric 1 at 100°C for drying and solidification to obtain an impregnated fabric; S2. Put the impregnated fabric obtained in step S1 into toluene for reduction, continue to soak for 2 hours, and finally dry the reduced impregnated fabric to obtain a corrosion-resistant and wear-resistant microfiber cloth.

[0067] [Example 3] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating and the preparation method are different.

[0068] In this embodiment, the modified polyurethane coating 2 is formed by double-sided impregnation and solidification of a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-3] on the island-in-sea non-woven fabric 1.

[0069] A method for preparing a corrosion-resistant and wear-resistant microfiber cloth comprises the following steps: S1, immersing the island-in-sea type nonwoven fabric 1 in a modified aqueous polyurethane immersion solution, controlling the liquid content to 100%, then scraping off excess modified aqueous polyurethane immersion solution on the surface, and placing the island-in-sea type nonwoven fabric 1 at 120° C. to dry and solidify, to obtain an impregnated fabric; S2. Put the impregnated base fabric obtained in step S1 into toluene for weight reduction, continue soaking for 3 hours, and finally dry the impregnated base fabric after weight reduction to obtain a corrosion-resistant and wear-resistant microfiber fabric.

[0070] [Example 4] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0071] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-4] on the island-in-sea non-woven fabric 1.

[0072] [Example 5] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0073] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-5] on the sea-island type non-woven base fabric 1.

[0074] [Example 6] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0075] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-6] on the island-in-sea non-woven fabric 1.

[0076] [Example 7] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0077] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-7] on the sea-island type non-woven base fabric 1.

[0078] [Example 8] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0079] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-8] on the sea-island type non-woven fabric 1.

[0080] [Example 9] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0081] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-4] on the island-in-sea non-woven fabric 1.

[0082] [Example 10] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0083] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-10] on the sea-island type non-woven fabric 1.

[0084] [Example 11] A corrosion-resistant and wear-resistant microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0085] In this embodiment, the modified polyurethane coating 2 is formed by impregnating and solidifying a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-11] on the sea-island type non-woven fabric 1.

[0086] Comparative Example [Comparative Example 1] A microfiber cloth is composed of an island-in-sea type nonwoven base fabric 1 and a polyurethane coating, wherein the polyurethane coating is formed by double-sided impregnation and solidification of a common solvent-based polyurethane on the market on the island-in-sea type nonwoven base fabric 1, and specifically the solvent-based polyurethane with the brand RG7530 is selected.

[0087] [Comparative Example 2] A microfiber cloth is composed of an island-in-sea type nonwoven base fabric 1 and a polyurethane coating, wherein the polyurethane coating is formed by double-sided impregnation and solidification of a common water-based polyurethane on the market on the island-in-sea type nonwoven base fabric 1, and the specific water-based polyurethane selected is PU-32K.

[0088] [Comparative Example 3] A microfiber cloth, which differs from [Example 1] in that the modified polyurethane coating 2 is different.

[0089] In this comparative example, the modified polyurethane coating 2 is formed by double-sided impregnation and coagulation of a modified aqueous polyurethane impregnation liquid prepared in [Preparation Example 2-12] on the island-in-sea nonwoven fabric 1.

[0090] Performance test data 1. Softness test: According to 6.3 of GB / T 39371-2020 Determination of softness of leather in physical and mechanical tests, the softness (mm) of the microfiber cloth prepared in each embodiment and comparative example is recorded. The higher the softness, the softer the texture of the microfiber cloth. The experimental conditions are standard atmosphere 23°C, 50% Rh, and the circular aperture of the metal ring is 25mm.

[0091] 2. Wear test: According to GB / T 30314-2021 Determination of wear resistance of rubber or plastic coated fabrics Taber, the test was carried out, and the average value (mg / r) of the mass loss of the microfiber cloth prepared in each embodiment and comparative example was recorded. Among them, the grinding wheel was CS10, and the load was 8N.

[0092] 3. Corrosion resistance test: According to 4.6.2 of "GB / T 40258-2021 Evaluation method for corrosion resistance of hollow fiber membranes to chemical cleaning agents", when preparing the samples, 0.05 g of phthalocyanine blue was added to the polyurethane immersion solution used in each embodiment and comparative example as an indicator color. After soaking for 24 hours, the appearance changes of each embodiment and comparative example were observed and recorded.

[0093] Table 1 Performance test data of microfiber cloth Combining Example 1 with Comparative Examples 1-2 and the data in Table 1, it can be seen that compared with Comparative Examples 1, 2 and 3, the polyurethane coating of Example 1 is formed by impregnation and solidification using a modified aqueous polyurethane immersion liquid, wherein the aqueous modified aqueous polyurethane immersion liquid used in Example 1 is added with a fluorosilicone solution containing terminal vinyl fluorosilicone oil and hydrogen fluorosilicone oil, and is mixed with specific diisocyanates, polyester polyols, polyether polyols, chain extenders and other additives in a specific proportion. The prepared microfiber cloth not only has good softness and wear resistance, but also has improved alkali corrosion resistance, and its comprehensive performance is close to that of the microfiber cloth prepared using solvent-based polyurethane in Comparative Example 1.

[0094] Combining Example 1 with Examples 4-6 and the data in Table 1, it can be seen that when the diisocyanate is selected from hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate in a weight ratio of 1: (1.5-2.5), compared with the use of hydrogenated diphenylmethane diisocyanate or isophorone diisocyanate alone, the microfiber cloth prepared by the modified aqueous polyurethane impregnation solution mixed with the two has better comprehensive performance, and as the proportion of isophorone diisocyanate increases, the softness of the microfiber cloth will be further improved, while the wear resistance will decrease slightly. Specifically, compared with the use of hydrogenated diphenylmethane diisocyanate alone, it has good softness, and when isophorone diisocyanate is used alone, although it has higher softness, the wear resistance of the obtained microfiber cloth is poor. This may be because hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate are both alicyclic isocyanates that can give polyurethane excellent mechanical strength and chemical corrosion resistance. The molecular structure of hydrogenated diphenylmethane diisocyanate tends to form an ordered arrangement and has a high degree of crystallinity, while isophorone diisocyanate has methyl side chains. Due to its molecular structure, it is not easy to crystallize or phase separate, and has a lower degree of crystallinity when forming polyurethane, thereby further improving the flexibility of polyurethane compared to hydrogenated diphenylmethane diisocyanate.

[0095] In conjunction with embodiment 6 and embodiment 7-8 and in conjunction with the data in table 1, when selecting polybutylene adipate diol and polytetrahydrofuran diol to mix according to the weight ratio of 1:(0.8-1) in the modified waterborne polyurethane immersion liquid, the softness of the obtained microfiber cloth can be further improved, and along with the polytetrahydrofuran diol content increase, the softness of the microfiber cloth also can be improved thereupon, and abrasion resistance can be reduced thereupon on a small amount. This may be because polybutylene adipate diol has higher crystallinity, is conducive to improving the mechanical strength of polyurethane, and the poor crystallinity of polytetrahydrofuran diol is conducive to improving the softness of polyurethane. Secondly, polybutylene adipate diol contains ester group, has higher polarity, may affect the dispersibility of polyurethane in water, and polytetrahydrofuran diol is due to the non-polarity of its ether parts, and polarity is lower, along with the polytetrahydrofuran diol proportion improves, is conducive to making polyurethane fully dispersed in aqueous solution, makes the modified waterborne polyurethane immersion liquid more uniform.

[0096] Combining Example 8 with Example 9 and the data in Table 1, it can be seen that when the chain extender in the modified waterborne polyurethane immersion solution is hydroxymethane and sodium dihydroxysulfonate mixed at a weight ratio of 1:1.5, the softness and wear resistance of the obtained microfiber cloth are further improved compared to when mixed at a weight ratio of 1:1. This may be because sodium dihydroxysulfonate is a hydrophilic chain extender, which is beneficial to improve the hydrophilicity of polyurethane during chain extension polymerization, making the modified polyurethane more evenly dispersed in water, and preventing undesirable phenomena such as macromolecular agglomeration.

[0097] Combining Examples 9-11 and the data in Table 1, it can be seen that when the hydrogen content of the hydrogen-containing fluorosilicone oil used in the fluorocarbon solution in the modified aqueous polyurethane immersion solution is gradually increased, the wear resistance of the obtained microfiber cloth will be further improved, but its softness will decrease. This may be because as the mass fraction of active hydrogen in the hydrogen-containing fluorosilicone oil increases, the crosslinking points on the molecular chain segments of the vinyl-terminated fluorosilicone oil increase, which in turn promotes further crosslinking of the vinyl-terminated fluorosilicone oil, thereby increasing the crosslinking density of the modified polyurethane coating, so that the hardness and strength of the microfiber cloth are improved, resulting in greatly improved wear resistance and reduced softness.

[0098] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A corrosion-resistant and wear-resistant microfiber cloth, characterized in that: The invention is composed of an island-in-sea type non-woven base fabric (1) and a modified polyurethane coating (2), wherein the modified polyurethane coating (2) is formed by impregnating a modified aqueous polyurethane impregnation liquid on both sides of the island-in-sea type non-woven base fabric (1) and solidifying the impregnation liquid, wherein the modified aqueous polyurethane impregnation liquid comprises the following raw materials: Diisocyanate: 100-120 parts; Polybutylene adipate diol: 120-180 parts; Polytetrahydrofuran diol: 90-120 parts; Trihydroxymethane: 10-20 parts; Sodium dihydroxysulfonate: 12-24 parts; Dimethylolpropionic acid: 8-12 parts; Triethylamine: 12-18 parts; Polypropylene glycol: 200-300 parts; 40-65 parts of fluorine silicon solution; Light stabilizer: 4.5-6 parts; Wherein, the diisocyanate comprises at least one of toluene diisocyanate, hydrogenated diphenylmethane diisocyanate and isophorone diisocyanate, the molecular weight of the polybutylene adipate diol is 1000-2000, and the molecular weight of the polytetrahydrofuran diol is 2000-3000.

2. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The fluorine silicon solution is prepared by mixing the following raw materials in parts by weight: Vinyl-terminated fluorosilicone oil: 100 parts; Hydrogen fluorinated silicone oil: 3.2-4.8 parts; Platinum catalyst: 0.48-0.64 parts; Compatibilizer: 4.5-8 parts.

3. The corrosion-resistant and wear-resistant microfiber cloth according to claim 2, characterized in that: The mass fraction of vinyl in the vinyl-terminated fluorosilicone oil is 1.2%-1.5%, and the mass fraction of active hydrogen in the hydrogen-containing fluorosilicone oil is 0.4%-0.6%.

4. The corrosion-resistant and wear-resistant microfiber cloth according to claim 2, characterized in that: The compatibilizer is prepared by mixing KH550 silane coupling agent and KH560 silane coupling agent in a weight ratio of 1: (0.8-1.2).

5. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The diisocyanate is a composite mixture of the hydrogenated diphenylmethane diisocyanate and the isophorone diisocyanate, and the mixing weight ratio of the hydrogenated diphenylmethane diisocyanate to the isophorone diisocyanate is 1:(1.5-2.5).

6. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The weight ratio of the polybutylene adipate diol to the polytetrahydrofuran diol is 1:(0.8-1).

7. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The weight ratio of the trihydroxymethane to the sodium dihydroxysulfonate is 1:(1-1.5).

8. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The light stabilizer is a mixture of UV-770 and UV-P in a weight ratio of 1: (0.5-0.6).

9. The corrosion-resistant and wear-resistant microfiber cloth according to claim 1, characterized in that: The method for preparing the modified aqueous polyurethane immersion liquid comprises the following steps: A1. First, polybutylene adipate diol, polytetrahydrofuran diol, trihydroxymethane and sodium dihydroxysulfonate are placed in a vacuum dehydration environment at 110-120° C., then fully stirred and mixed, cooled to 58-62° C. and added with diisocyanate, stirred evenly and then slowly heated to 65-76° C. and continued to react for 1-2 hours, then polypropylene glycol was added and continued to react for 1-2 hours to obtain a polyurethane prepolymer; A2. Cool the polyurethane prepolymer obtained in step A1 to 50-55° C., then add dimethylolpropionic acid, triethylamine, fluorine silicon solution and light stabilizer while stirring, and keep stirring the reaction for 2-3 hours. Finally, use deionized water for high-speed dispersion and emulsification to obtain a modified waterborne polyurethane immersion liquid.

10. A corrosion-resistant and wear-resistant microfiber cloth and a preparation method thereof, characterized in that: The method for preparing the corrosion-resistant and wear-resistant microfiber cloth according to any one of claims 1 to 9 comprises the following steps: S1, immersing the island-in-sea type nonwoven fabric (1) in a modified waterborne polyurethane impregnation liquid, controlling the liquid content to 85%-100%, then scraping off excess modified waterborne polyurethane impregnation liquid on the surface, and placing the island-in-sea type nonwoven fabric (1) at 100-120° C. to dry and solidify, thereby obtaining an impregnated fabric; S2. Put the impregnated base fabric obtained in step S1 into toluene for weight reduction, continue soaking for 2-3 hours, and finally dry the impregnated base fabric after weight reduction to obtain a corrosion-resistant and wear-resistant microfiber fabric.