Trimming V belt

By optimizing the rubber composition and structure in the cutting edge V belt, the transmission ratio changes in the time and the appropriate maintenance of the shaft load during high load transmission are achieved, and the transmission ratio changes and shaft load problems in the prior art are solved, thereby improving the Transmission efficiency and temperature control.

CN119084546APending Publication Date: 2024-12-06BANDO CHEM IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410685985.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2024-05-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing cutting edge V-band is difficult to suppress the time-lapse change of the transmission ratio during high load transmission, while maintaining the shaft load within an appropriate range, affecting the increase in transmission efficiency and belt temperature.

Method used

The rubber-made edge V-band has a compression elastic modulus of more than 150MPa and less than 250MPa, a 90° friction coefficient of more than 1.4 and less than 1.8, and a double-tooth structure with multiple teeth on the inner and outer sides of the belt is provided by Optimize the structure of the rubber composition and core wire, reduce the elapsed time variation of the transport ratio and maintain the axial load within the appropriate range.

Benefits of technology

The transmission ratio changes in the time of transmission during high load transmission are achieved, the shaft load is maintained within an appropriate range, the transmission efficiency is sufficient, and the belt temperature is not easy to rise, showing good performance balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119084546A_ABST
    Figure CN119084546A_ABST
Patent Text Reader

Abstract

A trimmed V-belt comprises: a rubber belt main body which forms pulley contact surfaces on both sides in the belt width direction; and a core wire embedded in the belt main body, in the trimmed V-belt, the compressive elastic modulus in the belt width direction measured at 120 DEG C is 150 MPa to 250 MPa, and the 90 DEG friction coefficient of the belt side surface is 1.4 to 1.8.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the priority based on Japanese Patent Application No. 2023-093343 for which it applied on June 6, 2023, and cites all the contents described in the said Japanese Patent Application. Technical Field

[0002] The invention relates to a cut-edge V-belt. Background Art

[0003] In belt-type continuously variable transmissions mounted on vehicles such as two-wheeled vehicles, buggies (all-terrain vehicles (ATV)), and snowmobiles, a raw edge V belt made of rubber is used as a transmission belt.

[0004] For example, Patent Document 1 discloses a double cogged V-belt in which a core wire having a shrinkage rate of 1.2% to 2.0% when heat-treated at 120° C. for one hour is buried in order to suppress a temporal change in transmission ratio.

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] [Patent Document 1] WO2015 / 121907 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] The cut edge V-belt for speed change is required to maintain the shaft load within an appropriate range while suppressing the change in the transmission ratio over time.

[0010] In particular, the cut edge V-belts used for speed change in buggy racing or snowmobiles are required to have such characteristics when transmitting high loads.

[0011] [Technical means to solve the problem]

[0012] The present invention has been made in view of such actual conditions, and an object of the present invention is to provide a cut edge V-belt having a small change in transmission ratio over time and capable of maintaining an axial load within an appropriate range.

[0013] (1) The trimmed V-belt of the present invention comprises:

[0014] A rubber belt body, which forms pulley contact surfaces on both sides in the belt width direction; and

[0015] A core wire is embedded in the belt body.

[0016] In the trimmed V-belt,

[0017] The compressive elastic modulus in the belt width direction measured at 120° C. is 150 MPa or more and 250 MPa or less,

[0018] The 90° friction coefficient of the belt side surface is 1.4 or more and 1.8 or less.

[0019] The cut edge V-belt can keep the shaft load within an appropriate range while suppressing the time variation of the transmission ratio. The cut edge V-belt can keep the shaft load within an appropriate range while suppressing the time variation of the transmission ratio even when transmitting high load.

[0020] In addition, the cut edge V-belt has sufficient power transmission efficiency and the belt temperature is unlikely to rise during running.

[0021] Therefore, the cut edge V-belt is a belt having extremely well-balanced properties.

[0022] (2) The cut edge V-belt is preferably a double-tooth V-belt having a plurality of teeth on the inner circumference side and the outer circumference side of the belt.

[0023] This is because the double-tooth V-belt for a belt-type continuously variable transmission is particularly required to keep the shaft load within an appropriate range while suppressing the temporal change of the transmission ratio.

[0024] [Effects of the Invention]

[0025] According to the present invention, it is possible to provide a cut edge V-belt which has a small change in transmission ratio over time and can maintain the shaft load within an appropriate range. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a perspective view schematically showing a part of a double-toothed V-belt according to an embodiment of the present invention.

[0027] Figure 2 yes Figure 1 A cross-sectional view of a double-tooth V-belt along the length of the belt.

[0028] Figure 3 This is a diagram for explaining a test piece for measuring the compressive elastic modulus.

[0029] Figure 4 This is a diagram for explaining a method for measuring the compressive elastic modulus.

[0030] Figure 5 This is a diagram for explaining the method of measuring the friction coefficient.

[0031] [Explanation of Symbols]

[0032] 10: Double tooth V belt

[0033] 11: With main body

[0034] 12: Core wire

[0035] 13: Reinforced cloth

[0036] 14: Lower teeth

[0037] 15: Upper teeth

[0038] 21: Load detector

[0039] 22, 25: Metal wire

[0040] 23: Pulley

[0041] 24: Heavy Hammer

[0042] 31: Side

[0043] 41: Lower plate (flat plate)

[0044] 42: Upper plate (flat plate)

[0045] 43: Axis

[0046] 111: Bonding rubber layer

[0047] 112: Compression rubber layer

[0048] 112a: Lower tooth forming portion

[0049] 113: Stretch rubber layer

[0050] HL, HU: Height

[0051] PL, PU: Installation spacing

[0052] T1, T2: Tension

[0053] TP: Test piece

[0054] WL, WU: Width

[0055] α: contact angle DETAILED DESCRIPTION

[0056] The following describes the embodiments of the present invention with reference to the accompanying drawings. The embodiments disclosed below are illustrative and non-restrictive in all aspects. The scope of the present invention is represented by the claims rather than the embodiments, and includes all changes within the scope of the structures equivalent to those described in the claims.

[0057] Figure 1 as well as Figure 2A double-toothed V-belt 10 (cut edge V-belt) according to an embodiment of the present invention is shown. The double-toothed V-belt 10 is a cut edge V-belt used as a power transmission member for speed change in a speed change device of, for example, an ATV or a snowmobile.

[0058] The double-toothed V-belt 10 is an endless transmission belt.

[0059] The length of the double-toothed V-belt 10 is, for example, 500 mm to 1400 mm, the maximum belt width is, for example, 15 mm to 40 mm, and the maximum belt thickness is, for example, 7.0 mm to 18.0 mm.

[0060] The double-toothed V-belt 10 includes a belt body 11 , a core wire 12 , and a reinforcing cloth 13 .

[0061] The belt main body 11 is made of rubber.

[0062] The shape of the cross section perpendicular to the belt length direction of the belt body 11 is a combination of a rectangular shape located on the outer circumference of the belt and a trapezoid located on the inner circumference of the belt and having a short bottom side on the inner circumference of the belt (see Figure 1 ).

[0063] The belt body 11 has inclined surfaces on both side surfaces. The inclined surfaces serve as pulley contact surfaces.

[0064] The belt body 11 is composed of three layers: an adhesive rubber layer 111 in the middle portion in the belt thickness direction, a compression rubber layer 112 on the inner peripheral side of the belt, and a tension rubber layer 113 on the outer peripheral side of the belt.

[0065] The core wire 12 is embedded in the middle portion in the belt thickness direction of the adhesive rubber layer 111. The core wire 12 is provided so as to extend in a spiral with a pitch in the belt width direction along the circumferential direction.

[0066] The reinforcing cloth 13 is provided so as to cover the surface of the compression rubber layer 112 on the belt inner peripheral side.

[0067] A plurality of lower tooth formations 112a are arranged at regular intervals along the belt length direction on the inner periphery of the compression rubber layer 112. The lower tooth formations 112a are provided so that the contour line of the inner periphery of the belt forms a sine curve in a cross section along the belt length direction.

[0068] A plurality of upper teeth 15 are arranged at regular intervals along the belt length direction on the outer periphery of the tension rubber layer 113. The cross-sectional shape of the upper teeth 15 in a cross section along the belt length direction is a substantially trapezoidal shape.

[0069] For example, the upper teeth 15 have a height HU of 2.0 mm to 5.0 mm, a width WU of 8.0 mm to 10.0 mm, and an arrangement pitch PU of 8.0 mm to 10.0 mm.

[0070] The adhesive rubber layer 111 , the compression rubber layer 112 , and the tension rubber layer 113 include a cross-linked product of an uncross-linked rubber composition obtained by mixing and kneading a rubber component with additives as necessary.

[0071] Examples of the rubber component include chloroprene rubber (CR), chlorosulfonated polyethylene rubber (CSM), hydrogenated acrylonitrile rubber (H-NBR), ethylene-α-olefin elastomer (EPDM), ethylene propylene rubber (EPR), etc.).

[0072] Among these, chloroprene rubber (CR) and ethylene-propylene-diene copolymer (EPDM) are preferred.

[0073] Examples of the additives include reinforcing materials, fillers, antioxidants, softeners, crosslinking agents, vulcanization accelerators, vulcanization accelerator aids, co-crosslinking agents, and processing aids.

[0074] The adhesive rubber layer 111 , the compression rubber layer 112 , and the tension rubber layer 113 may be formed using the same rubber composition or may be formed using different rubber compositions.

[0075] The compression rubber layer 112 and the tension rubber layer 113 may contain short fibers as reinforcement. When the short fibers are contained, the short fibers are preferably oriented in the belt width direction. By orienting the short fibers in the belt width direction, the rigidity in the belt width direction can be increased.

[0076] The core wire 12 is embedded in the middle portion in the thickness direction of the adhesive rubber layer 111 of the belt body 11. The core wire 12 is provided with a pitch in the belt width direction and is formed into a spiral.

[0077] The outer diameter of the core wire 12 in the tape width direction is preferably 0.7 mm or more and 1.3 mm or less, and more preferably 0.9 mm or more and 1.1 mm or less.

[0078] The arrangement pitch of the core wires 12 in the tape width direction is preferably 1.30 mm or less, more preferably 1.25 mm or less, and even more preferably 1.20 mm or less.

[0079] The arrangement pitch of the core wires 12 in the tape width direction refers to the distance between the centers of the adjacent core wires 12 in the tape width direction.

[0080] The core wire 12 is composed of twisted yarns. Examples of the fibers constituting the twisted yarns include polyester fibers, polyethylene naphthalate fibers, aramid fibers, and vinylon fibers.

[0081] It is preferable to perform bonding treatment on the core wire 12. By performing bonding treatment, it is possible to improve the bonding strength with the bonding rubber layer 111. The bonding treatment is performed before the molding process.

[0082] As the bonding treatment, the bonding treatment may be: a bonding treatment in which the substrate is immersed in a base treatment agent containing an epoxy compound or an isocyanate compound and then heated, a bonding treatment in which the substrate is immersed in a resorcinol formaldehyde latex (RFL) aqueous solution and then heated, a bonding treatment in which the substrate is immersed in a rubber paste and then dried, etc. These bonding treatments may be performed alone or in combination of two or more.

[0083] The reinforcing cloth 13 is provided to cover the inner peripheral surface of the compression rubber layer 112 of the belt body 11. The lower teeth forming portion 112a of the compression rubber layer 112 is covered with the reinforcing cloth 13, and the lower teeth 14 are formed by the lower teeth forming portion 112a and the reinforcing cloth 13.

[0084] Regarding the lower teeth 14 , for example, the height HL is 4.0 mm or more and 8.0 mm or less, the width WL is 8.0 mm or more and 12.0 mm or less, and the arrangement pitch PL is 8.0 mm or more and 12.0 mm or less.

[0085] The thickness of the reinforcing cloth 13 is, for example, not less than 0.1 mm and not more than 1.0 mm.

[0086] The reinforcing cloth 13 is generally made of woven cloth or knitted cloth. Examples of the fiber material constituting the reinforcing cloth 13 include aliphatic polyamide fibers, aramid fibers, polyester fibers, and cotton.

[0087] From the viewpoint of improving the adhesiveness to the compression rubber layer 112 , the reinforcing cloth 13 is preferably subjected to an adhesive treatment before being bonded to the compression rubber layer 112 .

[0088] As the bonding treatment, for example, the following can be adopted: a bonding treatment in which the tape is immersed in a base treatment agent containing an epoxy compound or an isocyanate compound and then heated; a bonding treatment in which the tape is immersed in an RFL aqueous solution and then heated; a bonding treatment in which the tape is immersed in a rubber paste and then dried; a bonding treatment in which a high-viscosity rubber paste is applied to the surface on the side of the belt body 11 and then dried; etc. These bonding treatments may be performed alone or in combination of two or more.

[0089] The double-toothed V-belt 10 has a compressive elastic modulus in the belt width direction measured at 120° C. of 150 MPa to 250 MPa, and a 90° friction coefficient of the belt side surface of 1.4 to 1.8.

[0090] The double-toothed V-belt 10 that satisfies the compression elastic modulus and the friction coefficient can reduce the time-dependent change of the transmission ratio and maintain the shaft load within an appropriate range regardless of whether it is a low-load transmission or a high-load transmission. In addition, the double-toothed V-belt 10 has sufficient transmission efficiency and the belt temperature is not easy to rise during travel.

[0091] The reason for measuring the compression modulus at 120° C. is that when the double-toothed V-belt 10 is used as a belt for a belt-type continuously variable transmission mounted on an ATV or a snowmobile, the temperature of the double-toothed V-belt 10 rises to about 120° C.

[0092] When the compressive elastic modulus is less than 150 MPa, the transmission ratio changes with time during high-load transmission due to buckling deformation of the double-toothed V-belt 10 and the like.

[0093] On the other hand, if the compression modulus exceeds 250 MPa, the shaft load may become too large and the burden on the shaft (the burden on the bearing supporting the shaft) may become too high, or the belt body 11 may become too hard and the heat generated when bent may become too large. In addition, the belt body 11 may be easily separated or cracked.

[0094] The compressive elastic modulus is preferably 200 MPa or more and 250 MPa or less.

[0095] When the 90° friction coefficient is less than 1.4, the time-dependent change of the transmission ratio during high-load transmission becomes large. In addition, the shaft load deteriorates. On the other hand, if the 90° friction coefficient exceeds 1.8, the belt temperature is likely to rise and the belt transmission efficiency is likely to decrease.

[0096] The 90° friction coefficient is more preferably 1.4 or more and 1.6 or less.

[0097] The shaft load is a load generated when the double-toothed V-belt is bridged between the driving shaft and the driven shaft.

[0098] The high shaft load means high belt tension. If the shaft load is too high, the load on the shaft becomes too high. In addition, the belt temperature is likely to rise, and the possibility of belt separation increases.

[0099] On the other hand, if the shaft load is too low, the belt tension is low and slip is likely to occur between the pulley and the belt, resulting in an increase in ratio variation or an increase in heat generation due to slip.

[0100] The shaft load is detected using a load cell.

[0101] The compressive elastic modulus is measured by the following method.

[0102] Figure 3 This is a diagram for explaining a test piece for measuring the compressive elastic modulus.

[0103] Figure 4 This is a diagram for explaining a method for measuring the compressive elastic modulus.

[0104] First, a cutting machine is used to cut out the double-toothed V-belt 10. Figure 4 Test piece TP as shown.

[0105] The dimensions of the test piece TP were set to length×width×thickness of four lower teeth×maximum belt thickness×40% of minimum belt width.

[0106] Here, the length of the test piece TP refers to the dimension in the belt length direction of the double-toothed V-belt 10. The width of the test piece TP refers to the dimension in the belt thickness direction of the double-toothed V-belt 10. In addition, the thickness of the test piece TP refers to the dimension in the belt width direction of the double-toothed V-belt 10.

[0107] The test piece TP is formed by cutting out the side surfaces of the double-toothed V-belt 10 so that the thickness dimension of the entire test piece TP is constant. Both side surfaces 31 of the test piece TP are parallel.

[0108] The compression modulus is measured using a fatigue / durability testing machine. As the fatigue / durability testing machine, a Servopulser manufactured by Shimadzu Corporation can be used.

[0109] The fatigue / endurance testing machine includes two flat plates for clamping the test piece TP. Figure 4 As shown in FIG. 1 , the two flat plates are composed of a lower plate 41 on which the test piece TP is placed, and an upper plate 42 fixed to a shaft 43 and movable up and down. The contact surface of each of the lower plate 41 and the upper plate 42 with the test piece TP has a size that can contact the entire lower surface or the entire upper surface of the test piece TP. The compression modulus is measured by sandwiching the test piece TP between the two flat plates 41 and 42, moving the upper plate 42 up and down, and applying a load to the entire upper surface of the test piece TP.

[0110] The test conditions were set as follows.

[0111] Load range: -1000N±500N

[0112] Frequency: 20Hz

[0113] Temperature: 120℃

[0114] Times: 3000 times

[0115] The compressive modulus was obtained at the 100th cycle, and further, values ​​were obtained in units of 100 cycles until the 3000th cycle. The average value of the obtained 30 values ​​was calculated and the obtained average value was used as the measured value of the compressive modulus.

[0116] The 90° friction coefficient is measured by the following method.

[0117] Figure 5 This is a diagram for explaining a method for measuring the friction coefficient of the double-toothed V-belt 10 .

[0118] First, the double-toothed V-belt 10 is cut at one position along the belt width direction. Next, one end of the double-toothed V-belt 10 is connected to a load detector 21 such as a weighing sensor via a metal wire 22. Then, the double-toothed V-belt 10 is wound around a pulley 23 having a groove of a shape corresponding to the double-toothed V-belt 10, and a weight 24 is hung from the other end of the double-toothed V-belt 10 via a metal wire 25, so that a downward load is applied to the double-toothed V-belt 10. Then, the pulley 23 is rotated in the counterclockwise direction at a predetermined speed, and the 90° friction coefficient μ of the belt side of the double-toothed V-belt 10 is measured by the following calculation formula.

[0119] μ=(1 / α)×ln(T1 / T2)

[0120] Wherein, T1 is the tension (N) measured by the load detector 21, T2 is the tension (N) generated by the weight 24 installed at the other end of the double-toothed V-belt 10, and α is the contact angle (rad) between the double-toothed V-belt 10 and the pulley 23.

[0121] In the measurement of the 90° friction coefficient, a pulley made of stainless steel (S45C) and having a pulley diameter of 96 mm was used as the pulley 23 .

[0122] The surface roughness Ra of the pulley 23 in contact with the double-toothed V-belt 10 is set to be 0.2 μm or more and 0.6 μm or less. The surface roughness Ra is the arithmetic mean roughness specified in Japanese Industrial Standards (JIS) B0601 (2013).

[0123] The tension generated by the weight 24 is set to 39.2N.

[0124] The rotation speed of the pulley 23 was set to 41 rpm.

[0125] The measurement time of the 90° friction coefficient was set to 30 seconds, and the highest value recorded from 5 seconds to 30 seconds after the start of the rotation of the pulley 23 was set as the measured value of the friction coefficient.

[0126] The atmospheric temperature during the measurement was set to 20°C to 25°C.

[0127] The determination of the cut edge V-belt by the compression elastic modulus and the 90° friction coefficient is more suitable for determining a cut edge V-belt that has a small change in transmission ratio over time and can maintain the shaft load within an appropriate range than the determination of the cut edge V-belt by the structure of the rubber composition and the structure of the cord. The reason for this is that the cut edge V-belt is determined based on the structure of the finished product.

[0128] The double-toothed V-belt 10 can reduce the temporal variation of the transmission ratio and maintain the shaft load within an appropriate range.

[0129] In addition, the double-toothed V-belt 10 has sufficient transmission efficiency and the belt temperature does not easily rise during running.

[0130] Therefore, the double-toothed V-belt 10 is a belt having extremely well-balanced performance.

[0131] The double-toothed V-belt 10 according to the embodiment of the present invention can be manufactured by a known method.

[0132] In the double-toothed V-belt 10 , only the inner peripheral surface of the compression rubber layer 112 is covered with the reinforcing cloth 13 , but the double-toothed V-belt according to the embodiment of the present invention is not limited thereto.

[0133] The double-toothed V-belt of the embodiment of the present invention may be a structure in which only the outer peripheral surface of the tension rubber layer 113 is covered with a reinforcing cloth. Alternatively, the inner peripheral surface of the compression rubber layer 112 and the outer peripheral surface of the tension rubber layer 113 may be covered with a reinforcing cloth. Furthermore, the inner peripheral surface of the compression rubber layer 112 and the outer peripheral surface of the tension rubber layer 113 may not be covered with a reinforcing cloth.

[0134] Herein, a double-toothed V-belt has been described as an embodiment of the present invention, but the cut-edge V-belt of the embodiment of the present invention is not limited thereto. The cut-edge V-belt of the embodiment of the present invention may be a single-toothed V-belt or a cut-edge V-belt without teeth.

[0135] [Example]

[0136] Hereinafter, the embodiments of the present invention will be described in more detail with reference to Examples, but the embodiments of the present invention are not limited to the following Examples.

[0137] (Double Tooth V-Belt)

[0138] Double-tooth V-belts of the following Examples 1 to 5 and Comparative Examples 1 to 5 were produced.

[0139] <Example 1 to Example 5>

[0140] A double-toothed V-belt having the same structure as the double-toothed V-belt 10 was manufactured.

[0141] As the rubber composition forming the adhesive rubber layer, the compression rubber layer, and the tension rubber layer, the same rubber composition is used.

[0142] Table 1 shows the structures of the rubber compositions used in Examples 1 to 5.

[0143] The core yarn is composed of twisted yarn of para-aramid fiber subjected to RFL treatment and rubber paste treatment.

[0144] The reinforcing fabric is composed of a woven fabric of aramid fiber subjected to RFL treatment and rubber paste treatment.

[0145] The double-toothed V-belts of Examples 1 to 5 have a belt length of 1100 mm, a maximum belt width of 32 mm, a maximum belt thickness of 16.5 mm, and an angle formed by the inclined surfaces constituting the pulley contact surfaces on both sides is 28°.

[0146] The adhesive rubber layer, the compression rubber layer, and the tensile rubber layer are formed of a rubber composition containing chloroprene rubber (CR) or ethylene-propylene-diene copolymer (EPDM) as a rubber component. The rubber composition forming the compression rubber layer and the tensile rubber layer contains aramid short fibers oriented in the belt width direction.

[0147] The lower teeth have a height HL of 7.0 mm, a width WL of 11.0 mm, and an arrangement pitch PL of 11.0 mm. The upper teeth have a height HU of 4.0 mm, a width WU of 9.0 mm, and an arrangement pitch PU of 9.0 mm.

[0148] The outer diameter of the core wire in the tape width direction is 1.0 mm, and the arrangement pitch of the core wire is 1.2 mm.

[0149] The pulley contact surfaces on both sides of the belt are formed by either grinding or cutting.

[0150]

[0151] <Comparative Examples 1 to 5>

[0152] A double-toothed V-belt was produced in the same manner as in the example except that the rubber composition for forming the adhesive rubber layer, the compression rubber layer, and the tension rubber layer was changed.

[0153] Table 2 shows the structures of the rubber compositions used in Comparative Examples 1 to 5.

[0154]

[0155] (Physical Property Evaluation)

[0156] The double-toothed V-belts produced in Examples and Comparative Examples were measured for compressive elastic modulus in the belt width direction at 120° C. and 90° friction coefficient of the belt side surface by the above-mentioned method.

[0157] In the measurement of the compressive elastic modulus, the dimensions of the test piece TP were set to 45 mm in length×10 mm in thickness×16.5 mm in width (see Figure 3 ).

[0158] The surface roughness Ra of the surface of the pulley 23 that contacts the double-toothed V-belt 10 is set to 0.2 μm.

[0159] The following evaluations (1) to (4) were performed. In the belt running test described below, the running test in which the drive shaft torque was set to 80 N·m was a running test during high load transmission.

[0160] (Performance Evaluation)

[0161] (1) Rate of change of ratio

[0162] Each double-toothed V-belt of Examples 1 to 5 and Comparative Examples 1 to 5 was wound around a drive pulley and a driven pulley with a variable winding diameter. The drive pulley was rotated at 2500 rpm to run the belt, and the input speed (N1) and output speed (N2) just after the belt started running, and the input speed (N1') and output speed (N2') when the drive shaft torque was set to 80 N·m were measured. The rate of change of the transmission ratio (ratio change rate) was calculated based on the following calculation formula. The results are shown in Table 3.

[0163] [Number 1]

[0164]

[0165] (2) Shaft load (N)

[0166] Use load cells to detect shaft loads as the belt travels.

[0167] Here, the belt was run under the same conditions as in the evaluation of the ratio change rate (1), and the drive shaft torque was set to 80 N·m. The shaft load was detected from 10 seconds to 30 seconds after the belt ran, and the average value was used as the result value. In addition, data sampling was performed at intervals of 200 milliseconds.

[0168] (3) Band temperature (℃)

[0169] In the evaluation of the ratio change rate (1), the belt temperature was measured using a non-contact type thermometer while the belt was running. The average value of the belt temperature when the drive shaft torque was maintained at 80 N·m for 30 seconds was taken as the result value. The results are shown in Table 3.

[0170] (4) Transmission efficiency (%)

[0171] Each double-toothed V-belt of Examples 1 to 5 and Comparative Examples 1 to 5 was wound around a drive pulley and a driven pulley with a variable winding diameter. The drive shaft torque was set to 80 N·m, and the drive pulley was rotated at 2500 rpm to advance the belt. The input speed (N1), input torque (Tr1), output speed (N2), and output torque (Tr2) were measured when the winding diameters of the drive pulley and the driven pulley were the same. The transmission efficiency was calculated based on the following calculation formula. The results are shown in Table 3.

[0172] [Number 2]

[0173]

[0174] (Performance evaluation results)

[0175] The evaluation results of the following (1) to (4) were scored according to the following criteria. The results are shown in Table 3. In the scoring, the larger the score, the higher the performance.

[0176] (1) Rate of change of ratio

[0177] 1 point: 8 or above

[0178] 2 points: 6 or more and less than 8

[0179] 3 points: less than 6

[0180] (2) Shaft load

[0181] 1 point: less than 2500N, or more than 4000N

[0182] 2 points: 2500N or more and less than 3000N, or 3500N or more and less than 4000N

[0183] 3 points: 3000N or more and less than 3500N

[0184] (3) With temperature

[0185] 1 point: above 60℃

[0186] 2 points: 53°C or higher and less than 60°C

[0187] 3 points: less than 53°C

[0188] It is considered that if the belt temperature is 60° C. or higher, it will have a significant influence on the reduction of the transmission efficiency and the reduction of the durability.

[0189] (4) Transmission efficiency

[0190] 1 point: less than 90%

[0191] 2 points: 90% or more and less than 92%

[0192] 3 points: above 92%

[0193] Then, based on the scores of each evaluation item, a comprehensive score was calculated by the following calculation formula.

[0194] Comprehensive score = (1) Ratio change rate score × 2 + (2) Axial load score × 2 + (3) Belt temperature score + (4) Transmission efficiency score

[0195] The present invention aims to provide a cut edge V-belt which can reduce the time-dependent change of the transmission ratio and maintain the shaft load within an appropriate range. In view of the above, in calculating the comprehensive score, the ratio change rate and the shaft load are weighted and evaluated compared with the belt temperature and the transmission efficiency.

[0196]

[0197] As is clear from the results shown in Table 3, the double-toothed V-belts of Examples 1 to 5 scored one or both of (1) ratio change rate and (2) axial load at 3 points, which is the highest score, and scored a total of 14 points or more.

[0198] On the other hand, the comprehensive scores of the double-toothed V-belts of Comparative Examples 1 to 5 were 13 points or less.

[0199] It is clear from this that the cut edge V-belt of the embodiment of the present invention is an excellent cut edge V-belt with well-balanced performance in terms of reducing the time-dependent change of the transmission ratio even during high-load transmission, maintaining the shaft load within an appropriate range, thereby suppressing the increase in belt temperature and ensuring sufficient transmission efficiency.

[0200] [Industrial Applicability]

[0201] The technology of the present invention can be used for cut edge V-belts.

Claims

1. A trimmed V-belt, comprising: A rubber belt body, which forms pulley contact surfaces on both sides in the belt width direction; as well as A core wire is embedded in the belt body. In the trimmed V-belt, The compressive elastic modulus in the belt width direction measured at 120° C. is 150 MPa or more and 250 MPa or less, The 90° friction coefficient of the belt side surface is 1.4 or more and 1.8 or less. 2 . The cut edge V-belt according to claim 1 , which is a double-tooth V-belt having a plurality of teeth on the inner circumference side and the outer circumference side of the belt.