A nanomaterial reinforced and toughened concrete

By using specially treated natural bamboo fibers and nanosilica nanocalcium carbonate composites in concrete, the problem of low mechanical properties of concrete under high temperature conditions is solved, the strength, toughness and durability are improved, and the high temperature building is broadened. Application in.

CN118851679BActive Publication Date: 2024-12-06SHANDONG HUABANG CONSTR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411350514.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-06
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

The low residual mechanical properties of existing concrete under high temperature or fire conditions limit its application in buildings that are resistant to high temperatures.

Method used

Using specially treated natural bamboo fibers and nanomaterials, including 5-sulfosalicylic acid-treated bamboo fibers and nanosilica nanocalcium carbonate composites, as raw materials components of concrete, the strength of concrete is improved by specific stirring and treatment methods. , toughness and durability.

Benefits of technology

The compressive strength, flexural strength, static compressive elastic modulus and split tensile strength of concrete are significantly improved, and the residual mechanical properties are maintained under different water-cement ratios and high temperature conditions are enhanced, and its durability is enhanced. Anti-compressed creep performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a nano-material reinforced toughened concrete, belonging to the field of concrete building materials. The raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite, and water reducer. The concrete of the invention has high residual mechanical properties, and can maintain high residual mechanical properties after being subjected to high temperature at different water-cement ratios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to nano material reinforced and toughened concrete, belonging to the field of concrete building materials. Background Art

[0002] Although concrete has become the world's largest man-made building material, its defects such as heavy weight, easy cracking, low tensile strength, small fracture strain value and brittle nature have not been fundamentally solved, its advantages cannot be fully utilized, and these defects also limit the better application of concrete structures under certain conditions.

[0003] From the current development status of concrete, it can be seen that concrete modification will be the main goal of future structural engineering research. The above-mentioned shortcomings of cement-based materials are essential and cannot be repaired by improving the material itself. They can only be solved through composite technical approaches.

[0004] Nano-scale mineral admixtures and fibers are typical concrete modification materials. They will significantly improve the original density, tensile and flexural strength of concrete, especially the toughness and impact resistance of concrete, thus changing the image of concrete in people's traditional concepts.

[0005] Nano-scale mineral admixtures have fine particles. On the one hand, they undergo secondary hydration reactions, and on the other hand, they fill the voids in concrete. Fiber materials have high tensile strength, which can complement each other's advantages and be used to improve the disadvantage of low tensile strength of concrete. Therefore, nano-scale mineral admixtures and fiber-reinforced concrete came into being, making the transformation of brittle concrete into elastic-ductile concrete.

[0006] During the solidification process of nano-scale mineral admixtures and cellulose fiber reinforced concrete, cellulose fibers can effectively reduce the number of cracks and refine the cracks. During the load process, cellulose has a bridging crack-blocking effect, delaying and inhibiting the cracking and expansion of cracks. Nano-scale mineral admixtures effectively improve the pore structure and compactness of concrete. Therefore, compared with ordinary plain concrete, nano-powder and cellulose reinforced concrete has excellent durability and can be widely used in houses, bridges, hydraulic engineering, tunnels and nuclear reactor protection buildings.

[0007] However, it was found in actual applications that the residual mechanical properties of nano-scale mineral admixtures and fiber concrete were low. After the concrete was affected by high temperature or fire, the cement gel began to dehydrate, and the water originally in chemical form began to be released and evaporated. Along with the continuous collapse of the gel structure, the average volume, surface area and porosity of the capillary pores began to increase, and microcracks gradually developed, causing the splitting tensile strength and compressive strength of the concrete to decrease, that is, the residual mechanical properties were low. During the experiment, it was found that by reducing the water-cement ratio of the concrete, the strength loss of the concrete at a temperature of 200°C can be reduced, and the residual mechanical properties are better, but it still cannot be solved under high temperature, which limits the application of concrete in buildings with fire and high temperature requirements. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the defects of the prior art. By specially treating natural bamboo fibers and nanomaterials and using them as raw material components of concrete, the strength and toughness of concrete can be significantly improved, and the durability of concrete can be improved. At the same time, the defect of low residual mechanical properties is avoided, and its application in buildings with fire and high temperature resistance requirements is broadened.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0010] A nano material reinforced toughened concrete, the raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano silicon oxide nano calcium carbonate composite, water reducing agent, the mass ratio of each component is 275-325:575-675:1170-1370:70-80:15-19:21-27:4.5-5.5.

[0011] The following are further improvements to the above technical solution:

[0012] The cement is 42.5R Portland cement;

[0013] The sand is river sand with an apparent density of 2390 kg / m 3 , the porosity is 43.5%, and the fineness modulus is 2.47;

[0014] The stone is mountain crushed stone, with continuous grading of 5-40mm and an apparent density of 2820kg / m 3 , porosity is 39.4%;

[0015] The fly ash is Class F fly ash, with an apparent density of 344 kg / m 3 , 45μm sieve residue is 5.2%, and loss on ignition is 1.74%;

[0016] The water reducer is a polycarboxylate water reducer, model number is PC-1007.

[0017] The preparation method of the 5-sulfosalicylic acid treated bamboo fiber is as follows:

[0018] The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and the stirring time is 45-55 minutes. After the stirring is completed, the pH is adjusted to 7.1-7.3, and then triethylamine is added, and the temperature is controlled to 72-77° C. The stirring is continued for 4.5-5.5 hours. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid-treated bamboo fiber;

[0019] The mass ratio of the bamboo fiber, deionized water, 5-sulfosalicylic acid and triethylamine is 65-75:275-325:45-55:0.9-1.1;

[0020] The bamboo fiber has a diameter of 13 μm, a length of 3.5 mm, and a density of 1.05 g / cm 3 , tensile strength is 737N / mm 2 .

[0021] The preparation method of the nano-silicon oxide and nano-calcium carbonate composite is as follows:

[0022] The temperature is controlled to be 610-630° C., the nano silicon dioxide is calcined for 125-175 min, and after the calcination is completed, the mixture is cooled to room temperature to obtain the calcined nano silicon dioxide, and the calcined nano silicon dioxide is mixed with a phosphoric acid solution and stirred for 20-30 min. After the stirring is completed, the mixture is filtered, washed, and dried. Then, the dried nano silicon dioxide, nano calcium carbonate, methyl titanium triisopropoxide, and methanol are mixed and stirred evenly, and ammonia water is used to adjust the pH value to 10.0-10.3, and then the mixture is aged in a nitrogen atmosphere for 5.5-6.5 h. After the aging is completed, the mixture is filtered, washed with methanol, and dried. The solid after filtration and drying is heated at a heating rate of 0.4-0.6° C. / min. When the temperature is increased to 770-815° C., the mixture is kept warm for 2.75-3.25 h. After the insulation is completed, the mixture is cooled to room temperature to obtain a nano silicon oxide nano calcium carbonate composite.

[0023] The mass ratio of the calcined nano-silicon dioxide to the phosphoric acid solution is 1:6.5-7.5;

[0024] The particle size of the nano-silicon dioxide is 54nm and the surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ;

[0025] The concentration of the phosphoric acid solution is 0.8-1.2 mol / L;

[0026] The mass ratio of the dried nano-silicon dioxide, nano-calcium carbonate, methyl titanium triisopropoxide, and methanol is 23-27:14-16:45-55:75-125;

[0027] The particle size of the nano calcium carbonate is 29 nm.

[0028] The preparation method of the concrete is:

[0029] The specified quantities of cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite and water reducing agent in the concrete raw material components are mixed uniformly to obtain nano-material reinforced and toughened concrete.

[0030] Compared with the prior art, the present invention achieves the following beneficial effects:

[0031] The concrete strength and toughness of the present invention are relatively excellent. According to the method in GB / T50081-2019, the compressive strength, axial compressive strength, flexural strength, static compressive elastic modulus, and splitting tensile strength of the concrete are tested, wherein the compressive strength is 47.6-48.5MPa, the axial compressive strength is 45.7-46.2MPa, the flexural strength is 9.27-9.44MPa, the static compressive elastic modulus is 45.8-46.4GPa, and the splitting tensile strength is 5.4-5.6MPa;

[0032] The concrete of the present invention has high slump and small slump change over time. According to the method in GB / T50080-2002, the initial slump and 1h slump of the concrete are tested, and the initial slump is 179-185mm, and the 1h slump is 176-180mm.

[0033] The concrete of the present invention has high residual mechanical properties. Under different water-cement ratios, the concrete can maintain relatively high residual mechanical properties after being subjected to high temperature. When the water-cement ratio is 0.38, the residual compressive strength at 200°C is 46.5-47.1MPa, the residual compressive strength at 400°C is 43.7-44.2MPa, the residual compressive strength at 600°C is 40.2-41.0MPa, and the residual compressive strength at 800°C is 37.3-37.5MPa; when the water-cement ratio is 0.40, the residual compressive strength at 200°C is The residual compressive strength at 400℃ is 43.2-43.5MPa, the residual compressive strength at 600℃ is 37.4-38.8MPa, and the residual compressive strength at 800℃ is 36.2-36.5MPa; when the water-cement ratio is 0.42, the residual compressive strength at 200℃ is 44.9-45.3MPa, the residual compressive strength at 400℃ is 42.9-43.1MPa, the residual compressive strength at 600℃ is 37.3-37.6MPa, and the residual compressive strength at 800℃ is 38.8MPa. The residual compressive strength at ℃ is 35.8-36.0MPa; when the water-cement ratio is 0.38, the residual splitting tensile strength at 200℃ is 5.3-5.4MPa, the residual splitting tensile strength at 400℃ is 4.7-5.0MPa, the residual splitting tensile strength at 600℃ is 4.4-4.6MPa, and the residual splitting tensile strength at 800℃ is 3.6-3.7MPa; when the water-cement ratio is 0.40, the residual splitting tensile strength at 200℃ is 5.0-5.3MPa, the residual splitting tensile strength at 400℃ is The tensile strength is 4.7-5.1MPa, the residual splitting tensile strength at 600℃ is 4.2-4.3MPa, and the residual splitting tensile strength at 800℃ is 3.5-3.7MPa; when the water-cement ratio is 0.42, the residual splitting tensile strength at 200℃ is 5.1-5.3MPa, the residual splitting tensile strength at 400℃ is 4.8-5.0MPa, the residual splitting tensile strength at 600℃ is 4.4-4.5MPa, and the residual splitting tensile strength at 800℃ is 3.4-3.6MPa;

[0034] The concrete of the present invention has good durability. According to the method in GB / T50082-2009, the water permeability resistance and chloride ion permeability resistance of the concrete are tested. The water permeability resistance adopts the water seepage height method, and the chloride ion permeability resistance adopts the electric flux method. The 28d water seepage height of the concrete is 1mm, and the 28d electric flux is 68-72C.

[0035] The concrete of the present invention has good anti-compressive creep performance. According to the method in GB / T50082-2009, the compressive creep of concrete is detected. The load of the creep test is controlled to be 500 kN. The creep degree of the specimen after 90 days of loading is 2.5×10 -6 MPa-2.7×10 -6 MPa, the creep of the specimen after 180d loading is 9.2×10 -6MPa-10.1×10 -6 MPa, and the creep of the specimen after 360 days of loading is 14.2×10 -6 MPa-15.4×10 -6 MPa. DETAILED DESCRIPTION Example 1

[0036] A nano-material reinforced toughened concrete, the raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite, water reducer, and the mass ratio of each component is 300:625:1270:75:17:24:5;

[0037] The cement is 42.5R Portland cement;

[0038] The sand is river sand with an apparent density of 2390 kg / m 3 , the porosity is 43.5%, and the fineness modulus is 2.47;

[0039] The stone is mountain crushed stone, with continuous grading of 5-40mm and an apparent density of 2820kg / m 3 , porosity is 39.4%;

[0040] The fly ash is Class F fly ash, with an apparent density of 344 kg / m 3 , 45μm sieve residue is 5.2%, and loss on ignition is 1.74%;

[0041] The water reducer is a polycarboxylate water reducer, model number is PC-1007.

[0042] The preparation method of the 5-sulfosalicylic acid treated bamboo fiber is as follows:

[0043] The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and the stirring time is 50 minutes. After the stirring is completed, the pH is adjusted to 7.2, and then triethylamine is added, and the temperature is controlled to 75° C. The stirring is continued for 5 hours. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid-treated bamboo fiber;

[0044] The mass ratio of the bamboo fiber, deionized water, 5-sulfosalicylic acid and triethylamine is 70:300:50:1;

[0045] The bamboo fiber has a diameter of 13 μm, a length of 3.5 mm, and a density of 1.05 g / cm 3 , tensile strength is 737N / mm 2 .

[0046] The preparation method of the nano-silicon oxide and nano-calcium carbonate composite is as follows:

[0047] The temperature is controlled to be 620°C, the nano silicon dioxide is calcined for 150 minutes, and after the calcination is completed, it is cooled to room temperature to obtain the calcined nano silicon dioxide, and the calcined nano silicon dioxide is mixed with a phosphoric acid solution and stirred for 25 minutes. After the stirring is completed, it is filtered, washed, and dried, and then the dried nano silicon dioxide, nano calcium carbonate, triisopropoxide methyl titanium, and methanol are mixed, and after stirring, ammonia water is used to adjust the pH to 10.2, and then it is aged in a nitrogen atmosphere for 6 hours. After the aging is completed, it is filtered, washed with methanol, and dried. The filtered and dried solid is heated at a heating rate of 0.5°C / min. When the temperature is raised to 785°C, it is kept warm for 3 hours. After the insulation is completed, it is cooled to room temperature to obtain a nano silicon oxide nano calcium carbonate composite;

[0048] The mass ratio of the calcined nano-silicon dioxide to the phosphoric acid solution is 1:7;

[0049] The particle size of the nano-silicon dioxide is 54nm and the surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ;

[0050] The concentration of the phosphoric acid solution is 1 mol / L;

[0051] The mass ratio of the dried nano-silicon dioxide, nano-calcium carbonate, methyl titanium triisopropoxide, and methanol is 25:15:50:100;

[0052] The particle size of the nano calcium carbonate is 29 nm.

[0053] The preparation method of the concrete is:

[0054] The specified quantities of cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite and water reducing agent in the concrete raw material components are mixed uniformly to obtain nano-material reinforced and toughened concrete. Example 2

[0055] A nano material reinforced toughened concrete, the raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano silicon oxide nano calcium carbonate composite, water reducing agent, the mass ratio of each component is 275:575:1170:70:15:21:4.5;

[0056] The cement is 42.5R Portland cement;

[0057] The sand is river sand with an apparent density of 2390 kg / m 3 , the porosity is 43.5%, and the fineness modulus is 2.47;

[0058] The stone is mountain crushed stone, with continuous grading of 5-40mm and an apparent density of 2820kg / m 3 , porosity is 39.4%;

[0059] The fly ash is Class F fly ash, with an apparent density of 344 kg / m 3 , 45μm sieve residue is 5.2%, and loss on ignition is 1.74%;

[0060] The water reducer is a polycarboxylate water reducer, model number is PC-1007.

[0061] The preparation method of the 5-sulfosalicylic acid treated bamboo fiber is as follows:

[0062] The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and the stirring time is 45 minutes. After the stirring is completed, the pH is adjusted to 7.1, and then triethylamine is added, the temperature is controlled to 72° C., and the stirring is continued for 5.5 hours. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid-treated bamboo fiber;

[0063] The mass ratio of the bamboo fiber, deionized water, 5-sulfosalicylic acid and triethylamine is 65:275:45:0.9;

[0064] The bamboo fiber has a diameter of 13 μm, a length of 3.5 mm, and a density of 1.05 g / cm 3 , tensile strength is 737N / mm 2 .

[0065] The preparation method of the nano-silicon oxide and nano-calcium carbonate composite is as follows:

[0066] The temperature is controlled to be 610°C, the nano-silicon dioxide is calcined for 175 minutes, and the calcination is completed and then cooled to room temperature to obtain the calcined nano-silicon dioxide, the calcined nano-silicon dioxide is mixed with a phosphoric acid solution, and the stirring time is 20 minutes. After the stirring is completed, it is filtered, washed, and dried, and then the dried nano-silicon dioxide, nano-calcium carbonate, triisopropylmethyl titanium, and methanol are mixed, and after stirring, the pH is adjusted to 10.0 with ammonia water, and then aged in a nitrogen atmosphere for 6.5 hours. After the aging is completed, it is filtered, washed with methanol, and dried. The filtered and dried solid is heated at a heating rate of 0.4°C / min. When the temperature is raised to 815°C, it is kept warm for 2.75 hours. After the insulation is completed, it is cooled to room temperature to obtain a nano-silicon oxide nano-calcium carbonate composite;

[0067] The mass ratio of the calcined nano-silicon dioxide to the phosphoric acid solution is 1:6.5;

[0068] The particle size of the nano-silicon dioxide is 54nm and the surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ;

[0069] The concentration of the phosphoric acid solution is 0.8 mol / L;

[0070] The mass ratio of the dried nano-silicon dioxide, nano-calcium carbonate, methyl titanium triisopropoxide, and methanol is 23:14:45:75;

[0071] The particle size of the nano calcium carbonate is 29 nm.

[0072] The preparation method of the concrete is:

[0073] The specified quantities of cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite and water reducing agent in the concrete raw material components are mixed uniformly to obtain nano-material reinforced and toughened concrete. Example 3

[0074] A nano-material reinforced toughened concrete, the raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite, water reducer, and the mass ratio of each component is 325:675:1370:80:19:27:5.5;

[0075] The cement is 42.5R Portland cement;

[0076] The sand is river sand with an apparent density of 2390 kg / m 3, the porosity is 43.5%, and the fineness modulus is 2.47;

[0077] The stone is mountain crushed stone, with continuous grading of 5-40mm and an apparent density of 2820kg / m 3 , porosity is 39.4%;

[0078] The fly ash is Class F fly ash, with an apparent density of 344 kg / m 3 , 45μm sieve residue is 5.2%, and loss on ignition is 1.74%;

[0079] The water reducer is a polycarboxylate water reducer, model number is PC-1007.

[0080] The preparation method of the 5-sulfosalicylic acid treated bamboo fiber is as follows:

[0081] The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and the stirring is performed for 55 minutes. After the stirring is completed, the pH is adjusted to 7.3, and then triethylamine is added, and the temperature is controlled to 77° C. The stirring is continued for 4.5 hours. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid-treated bamboo fiber;

[0082] The mass ratio of the bamboo fiber, deionized water, 5-sulfosalicylic acid and triethylamine is 75:325:55:1.1;

[0083] The bamboo fiber has a diameter of 13 μm, a length of 3.5 mm, and a density of 1.05 g / cm 3 , tensile strength is 737N / mm 2 .

[0084] The preparation method of the nano-silicon oxide and nano-calcium carbonate composite is as follows:

[0085] The temperature is controlled to be 630°C, the nano-silicon dioxide is calcined for 125 minutes, and the calcination is completed and then cooled to room temperature to obtain calcined nano-silicon dioxide, the calcined nano-silicon dioxide is mixed with a phosphoric acid solution, and the stirring time is 30 minutes. After the stirring is completed, it is filtered, washed, and dried, and then the dried nano-silicon dioxide, nano-calcium carbonate, triisopropylmethyl titanium, and methanol are mixed, and after stirring, ammonia water is used to adjust the pH to 10.3, and then aged in a nitrogen atmosphere for 5.5 hours. After the aging is completed, it is filtered, washed with methanol, and dried. The filtered and dried solid is heated at a heating rate of 0.6°C / min. When the temperature is raised to 770°C, it is kept warm for 3.25 hours. After the insulation is completed, it is cooled to room temperature to obtain a nano-silicon oxide nano-calcium carbonate composite;

[0086] The mass ratio of the calcined nano-silicon dioxide to the phosphoric acid solution is 1:7.5;

[0087] The particle size of the nano-silicon dioxide is 54nm and the surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ;

[0088] The concentration of the phosphoric acid solution is 1.2 mol / L;

[0089] The mass ratio of the dried nano-silicon dioxide, nano-calcium carbonate, methyl titanium triisopropoxide, and methanol is 27:16:55:125;

[0090] The particle size of the nano calcium carbonate is 29 nm.

[0091] The preparation method of the concrete is:

[0092] The specified quantities of cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite and water reducing agent in the concrete raw material components are mixed uniformly to obtain nano-material reinforced and toughened concrete.

[0093] Comparative Example 1

[0094] Different from Example 1, the preparation method of 5-sulfosalicylic acid treated bamboo fiber is changed to the following operation:

[0095] The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and stirred for 50 minutes. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid treated bamboo fiber.

[0096] The mass ratio of the bamboo fiber, deionized water and 5-sulfosalicylic acid is 70:300:50;

[0097] The bamboo fiber has a diameter of 13 μm, a length of 3.5 mm, and a density of 1.05 g / cm 3 , tensile strength is 737N / mm 2 ;

[0098] The proportion of 5-sulfosalicylic acid treated bamboo fiber in the raw materials was kept unchanged and the other steps were the same to prepare concrete.

[0099] Comparative Example 2

[0100] Different from Example 1, the preparation method of the nano-silicon oxide and nano-calcium carbonate composite is changed to the following operation:

[0101] The temperature is controlled to be 620° C., nano silicon dioxide and nano calcium carbonate are mixed and calcined for 150 minutes. After the calcination is completed, the mixture is cooled to room temperature to obtain calcined nano powders. The calcined nano powders are mixed with a phosphoric acid solution and stirred for 25 minutes. After the stirring is completed, the mixture is filtered, washed and dried to obtain a nano silicon oxide nano calcium carbonate composite.

[0102] The mass ratio of the nano-silicon dioxide to the nano-calcium carbonate is 2:1;

[0103] The mass ratio of the calcined nanopowder to the phosphoric acid solution is 3:20;

[0104] The particle size of the nano-silicon dioxide is 54nm and the surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ;

[0105] The concentration of the phosphoric acid solution is 1 mol / L;

[0106] The particle size of the nano calcium carbonate is 29 nm;

[0107] The proportion of nano-silicon oxide and nano-calcium carbonate composite in the raw materials is kept unchanged, and the remaining steps are the same to prepare concrete.

[0108] Test Example 1 Concrete strength and toughness test

[0109] The concrete of Examples 1-3 and Comparative Examples 1-2 was prepared according to the method in GB / T50081-2019 with a water-cement ratio of 0.42, and the compressive strength, axial compressive strength, flexural strength, static compressive elastic modulus, and splitting tensile strength of the concrete were tested according to the method in GB / T50081-2019. The results are shown in Table 1.

[0110] Table 1

[0111]

[0112] In Examples 1-3, natural bamboo fibers and nanomaterials are specially treated and used as raw material components of concrete. The concrete finally obtained has high strength and toughness, and has high compressive strength, axial compressive strength, flexural strength, static compressive elastic modulus, and splitting tensile strength.

[0113] In Comparative Example 1, only 5-sulfosalicylic acid was used to treat the bamboo fiber in one step, and the strength and toughness of the concrete finally obtained were relatively low, especially the splitting tensile strength decreased more seriously, and the compressive strength, axial compressive strength, flexural strength, and static compressive elastic modulus decreased to a certain extent;

[0114] In Comparative Example 2, nano-silicon dioxide and nano-calcium carbonate were mixed and calcined and then treated with phosphoric acid. The two were simply composited and the strength and toughness of the concrete finally obtained were low. The compressive strength, axial compressive strength, flexural strength, and static compressive elastic modulus decreased more seriously, and the splitting tensile strength decreased to a certain extent.

[0115] Test Example 2 Concrete Slump Test

[0116] The concrete of Examples 1-3 and Comparative Examples 1-2 were prepared according to the method in GB / T50080-2002 with a water-cement ratio of 0.42. The initial slump and 1h slump of the concrete were tested according to the method in GB / T50080-2002. The results are shown in Table 2.

[0117] Table 2

[0118]

[0119] In Examples 1-3, natural bamboo fiber and nanomaterials are specially treated and used as raw material components of concrete. The concrete finally obtained has a high slump, a small slump loss, and a high slump after 1h.

[0120] In Comparative Example 1, only 5-sulfosalicylic acid was used to treat the bamboo fiber in one step, and the slump of the concrete finally obtained was slightly reduced, but the slump loss was large, and the slump decreased greatly after 1h;

[0121] In Comparative Example 2, nano-silicon dioxide and nano-calcium carbonate were mixed and calcined and then treated with phosphoric acid. The two were simply composited. Although the slump loss of the concrete finally obtained was small, as shown by a small decrease in slump after 1 hour, the initial slump was low.

[0122] Test Example 3 Residual Mechanical Properties of Concrete at Different Water-Cement Ratios

[0123] The concrete of Examples 1-3 and Comparative Examples 1-2 were prepared with water-cement ratios of 0.38, 0.40, and 0.42, respectively. The specifications of the samples were 100 mm × 100 mm × 100 mm. After the sample preparation and curing were completed, the sample was first placed in a constant temperature oven at 120°C to heat the sample to evaporate the water inside the sample. The heating time was 180 minutes. After the heating was completed, the residual mechanical properties test process was carried out. The test method is as follows:

[0124] The sample was heated at a rate of 2°C / min. The samples with different water-cement ratios in each embodiment and comparative example were heated to 200°C, 400°C, 600°C, and 800°C, respectively, and then kept constant at different temperatures for 120 minutes. After the constant temperature was completed, the sample was cooled at room temperature. After the sample was cooled to room temperature, it was left to stand for 3 days before the residual mechanical properties were tested.

[0125] The method of residual mechanical properties test is as follows:

[0126] According to the method in GB / T50081-2019, the compressive strength, i.e. the residual compressive strength, is tested, and the results are shown in Table 3;

[0127] According to the method in GB / T50081-2019, the splitting tensile strength, i.e. the residual splitting tensile strength, was tested. The results are shown in Table 4.

[0128] Table 3 Unit: MPa

[0129]

[0130] Table 4 Unit: MPa

[0131]

[0132] In Examples 1-3, natural bamboo fibers and nanomaterials are specially treated and used as raw material components of concrete. The concrete finally obtained has high residual mechanical properties. At different water-cement ratios and in high-temperature environments at different temperatures, high residual compressive strength and residual splitting tensile strength can be maintained.

[0133] In Comparative Example 1, only 5-sulfosalicylic acid was used to treat the bamboo fiber in one step, and the residual mechanical properties of the concrete finally obtained were low. With the increase of water-cement ratio and temperature, the residual compressive strength and residual splitting tensile strength decreased significantly.

[0134] In Comparative Example 2, nano-silicon dioxide and nano-calcium carbonate were mixed and calcined and then treated with phosphoric acid. The two were simply composited and the residual mechanical properties of the concrete finally obtained were low. With the increase of water-cement ratio and temperature, the residual compressive strength and residual splitting tensile strength both decreased seriously.

[0135] Test Example 4 Concrete Durability Test

[0136] The concrete of Examples 1-3 and Comparative Examples 1-2 were prepared according to the method in GB / T50082-2009 with a water-cement ratio of 0.42. The concrete was tested for water permeability and chloride ion permeability according to the method in GB / T50082-2009. The water permeability was measured using the water seepage height method, and the chloride ion permeability was measured using the electrical flux method. The results are shown in Table 5.

[0137] Table 5

[0138]

[0139] In Examples 1-3, natural bamboo fibers and nanomaterials are specially treated and used as raw material components of concrete. The concrete finally prepared has high durability, high water permeability resistance and high chloride ion permeability resistance.

[0140] In Comparative Example 1, only 5-sulfosalicylic acid was used to treat the bamboo fiber in one step, and the durability of the concrete finally obtained was poor, wherein the water seepage resistance decreased more seriously, the water seepage height at 28 days was higher, and the chloride ion permeability resistance also decreased to a certain extent;

[0141] In Comparative Example 2, nano-silicon dioxide and nano-calcium carbonate were mixed and calcined and then treated with phosphoric acid. The two were simply composited and the durability of the concrete finally obtained was poor, among which the chloride ion permeability decreased more seriously, the 28d electrical flux was high, and the water seepage resistance also decreased to a certain extent.

[0142] Test Example 5: Concrete compression creep performance test

[0143] The concrete of Examples 1-3 and Comparative Examples 1-2 were prepared according to the method in GB / T50082-2009 with a water-cement ratio of 0.42. The compressive creep of the concrete was tested according to the method in GB / T50082-2009. The load of the creep test was controlled to be 500 kN. The creep of the specimens was measured at 90 d, 180 d, and 360 d after loading. The results are shown in Table 6.

[0144] Table 6

[0145]

[0146] In Examples 1-3, natural bamboo fibers and nanomaterials are specially treated and used as raw material components of concrete. The concrete finally obtained has high compressive creep resistance and can still maintain a low creep degree as the load time increases.

[0147] In Comparative Example 1, only 5-sulfosalicylic acid was used to treat the bamboo fiber in one step, and the resulting concrete had poor compressive creep resistance, and the creep degree increased more seriously with the increase of loading time;

[0148] In Comparative Example 2, nano-silicon dioxide and nano-calcium carbonate were mixed and calcined and then treated with phosphoric acid. The two were simply composited and the resulting concrete had poor compressive creep resistance. As the load time increased, the creep rate increased more seriously.

Claims

1. A nanomaterial reinforced and toughened concrete, characterized in that: The raw material components of the concrete include cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite, and water reducer, and the mass ratio of each component is 275-325:575-675:1170-1370:70-80:15-19:21-27:4.5-5.5; The preparation method of the 5-sulfosalicylic acid treated bamboo fiber is as follows: The bamboo fiber is mixed with deionized water, stirred to be evenly dispersed, and a dispersion of the bamboo fiber is obtained. Then, 5-sulfosalicylic acid is added to the bamboo fiber dispersion, and the stirring time is 45-55 minutes. After the stirring is completed, the pH is adjusted to 7.1-7.3, and then triethylamine is added, and the temperature is controlled to 72-77° C. The stirring is continued for 4.5-5.5 hours. After the stirring is completed, the bamboo fiber is filtered, washed, and dried to obtain 5-sulfosalicylic acid-treated bamboo fiber; The mass ratio of the bamboo fiber, deionized water, 5-sulfosalicylic acid and triethylamine is 65-75:275-325:45-55:0.9-1.1; The preparation method of the nano-silicon oxide and nano-calcium carbonate composite is as follows: The temperature is controlled to be 610-630° C., the nano silicon dioxide is calcined for 125-175 min, and after the calcination is completed, the mixture is cooled to room temperature to obtain the calcined nano silicon dioxide, and the calcined nano silicon dioxide is mixed with a phosphoric acid solution and stirred for 20-30 min. After the stirring is completed, the mixture is filtered, washed, and dried. Then, the dried nano silicon dioxide, nano calcium carbonate, methyl titanium triisopropoxide, and methanol are mixed and stirred evenly, and ammonia water is used to adjust the pH value to 10.0-10.3, and then the mixture is aged in a nitrogen atmosphere for 5.5-6.5 h. After the aging is completed, the mixture is filtered, washed with methanol, and dried. The solid after filtration and drying is heated at a heating rate of 0.4-0.6° C. / min. When the temperature is increased to 770-815° C., the mixture is kept warm for 2.75-3.25 h. After the insulation is completed, the mixture is cooled to room temperature to obtain a nano silicon oxide nano calcium carbonate composite. The mass ratio of the calcined nano-silicon dioxide to the phosphoric acid solution is 1:6.5-7.5; The concentration of the phosphoric acid solution is 0.8-1.2 mol / L; The mass ratio of the dried nano-silicon dioxide, nano-calcium carbonate, methyl titanium triisopropoxide and methanol is 23-27:14-16:45-55:75-125.

2. The nano-material reinforced and toughened concrete according to claim 1, characterized in that: The raw material components of the concrete include 42.5R Portland cement as cement and river sand with an apparent density of 2390 kg / m 3 The porosity is 43.5%, the fineness modulus is 2.47; the stone is mountain crushed stone, 5-40mm continuous grading, and the apparent density is 2820kg / m 3 The porosity is 39.4%; the fly ash is Class F fly ash, and the apparent density is 344kg / m 3 , the 45μm sieve residue is 5.2%, and the ignition loss is 1.74%.

3. The nano-material reinforced and toughened concrete according to claim 1, characterized in that: Among the raw material components of the concrete, the water reducer is a polycarboxylate water reducer, model number is PC-1007.

4. The nano-material reinforced and toughened concrete according to claim 1, characterized in that: In the preparation method of 5-sulfosalicylic acid treated bamboo fiber, the diameter of the bamboo fiber is 13 μm, the length is 3.5 mm, and the density is 1.05 g / cm 3 , tensile strength is 737N / mm 2 .

5. The nano-material reinforced and toughened concrete according to claim 1, characterized in that: In the preparation method of the nano-silicon oxide and nano-calcium carbonate composite, the particle size of the nano-silicon dioxide is 54nm and the specific surface area is 235m 2 / g, bulk density is 1.671g / cm 3 ; The particle size of nano calcium carbonate is 29nm.

6. The nano-material reinforced and toughened concrete according to claim 1, characterized in that: The preparation method of the concrete is to uniformly mix cement, sand, gravel, fly ash, 5-sulfosalicylic acid treated bamboo fiber, nano-silicon oxide nano-calcium carbonate composite and water reducer in specified quantities among the concrete raw material components to obtain nano-material reinforced and toughened concrete.