Indium oxide-based gas sensitive material as well as preparation method and application thereof
By adding Ag nanoparticles to the surface of alumina composite indium oxide nanorods and coating them with polyaniline, the prepared indium oxide-based gas-sensitive materials solve the problems of easy poisoning and production complexity of existing gas-sensitive materials, and realize the paraformaldehyde The high sensitivity and selective detection of gases are suitable for widespread use and reduce costs.
Patent Information
- Application Number
- CN202411006097.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-12-06
AI Technical Summary
Existing gas-sensitive materials are prone to poisoning when detecting formaldehyde gas, and the production process is complex and the conditions are harsh, so they are not suitable for large-scale production, and the working temperature is high, which poses safety hazards.
By using the preparation method of indium oxide-based gas-sensitive materials, by adding Ag nanoparticles to the surface of alumina composite indium oxide nanorods and carrying out polyaniline coating, the adsorption capacity and response speed of the material are enhanced, and the formaldehyde gas is contacted with the material is reduced. The activation energy barrier increases the sensitivity and selectivity to formaldehyde gas.
It realizes high sensitivity and selective detection of formaldehyde gas, simplifies the production process, reduces the cost of raw materials, is suitable for widespread use, and improves the long-term stability of the material.
Smart Images

Figure CN119086655A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of gas-sensitive material preparation, and in particular to an indium oxide-based gas-sensitive material and a preparation method and application thereof. Background Art
[0002] Formaldehyde gas is a protoplasmic poison that is long-term, latent, and hidden in its harm to human health. Human exposure to a certain concentration of formaldehyde can cause gastrointestinal corrosion, stomatitis, and esophageal inflammation. Repeated exposure to formaldehyde can easily cause nasal and laryngeal cancers. Formaldehyde and benzene produced by decoration are listed as Class I carcinogens by the World Health Organization (WHO). The detection and treatment of formaldehyde and other gases in confined spaces such as indoors and in cars are increasingly attracting people's attention.
[0003] Semiconductor oxide sensors are the most widely used type of gas sensors. When semiconductor oxide sensitive materials are used for formaldehyde gas detection, they are generally based on the redox reaction between formaldehyde gas molecules and oxygen species adsorbed on the surface of the sensitive material. The specific surface area of the metal oxide can be increased by surface functionalization or regulation of the nanostructure, thereby improving its sensitivity. Patent No. 200610042039.5 discloses a superimposed sensitive layer formaldehyde gas sensor and its manufacturing method. It adopts a side-heated device structure, uses an Al2O3 ceramic tube as a carrier, uses a comb-shaped Au electrode on the outer surface, and is doped with SnSO4 and AuCl3. The material of the outer surface thin film sensitive layer is an indium tin oxide nanofilm. Although it has the advantages of high sensitivity to formaldehyde gas, high resolution, good selectivity, and short response and recovery time, the amount of organic gas adsorbed after auxiliary heating is too large, which can easily lead to poisoning of the gas sensitive material, thereby affecting the stability of the gas sensor. The Chinese patent with publication number CN1804609A discloses a stacked sensitive layer formaldehyde gas sensor and its manufacturing method. Although it has the advantages of high sensitivity to formaldehyde gas, good anti-interference, short response time and recovery time, etc., the manufacturing process is complicated and the manufacturing conditions are harsh. It is not easy to mass produce. The working temperature of the gas sensor is high (260℃-300℃), and there are also safety hazards. Summary of the invention
[0004] In order to solve the above technical problems and develop a gas-sensitive material with high sensitivity, good selectivity and wide application, the present application provides an indium oxide-based gas-sensitive material and a preparation method and application thereof.
[0005] In a first aspect, the present application provides a method for preparing an indium oxide-based gas-sensitive material, comprising the following steps: S1. Add indium salt, aluminum salt, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction container, mix, stir, heat to 180-210° C., react for 24-36 hours, cool to room temperature, wash and centrifuge the precipitate, and dry to obtain a precursor powder; S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 into deionized water, mixing, stirring, dropping NaBH4 solution, ultrasonically dispersing to obtain a suspension, filtering, washing the filter residue, drying, and calcining at a high temperature of 500-650° C. for 2-4 h to obtain aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles; S3. Add the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods obtained in step S2 into deionized water, add aniline monomer, disperse by ultrasonication, cause copolymerization, react for 12-18 hours, filter, wash the filter residue, and dry to obtain an indium oxide-based gas-sensitive material.
[0006] By adopting the above technical solution, the energy difference between the Al-doped In2O3 nanorods and oxygen molecules becomes larger, so that the surface of the gas-sensitive material can increase the adsorption of oxygen atoms, thereby promoting the response of the prepared indium oxide-based gas-sensitive material to the detected gas. Ag nanoparticles are tightly adsorbed on the surface of the indium oxide nanorods. Ag nanoparticles can act as highly active catalysts on the surface of the indium oxide nanorods, produce more active sites, enhance the adsorption of oxygen molecules, and improve the performance of the gas-sensitive material through chemical sensitization caused by the overflow effect; in addition, Ag nanoparticles can also improve the gas-sensitive characteristics of the sensor by accelerating the gas-sensitive reaction and the electron transfer between the In2O3 matrix material. The combination of chemical sensitization and electronic sensitization makes it have a higher responsiveness. In addition, the present application coats the organic material polyaniline on the surface of aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles by in-situ polymerization, which can reduce the activation energy barrier of the reaction when formaldehyde gas contacts the gas-sensitive material, promote the reaction between formaldehyde gas and the adsorbed oxygen on the surface of the gas-sensitive material, and make the electrons captured by the adsorbed oxygen return to the conduction band of the gas-sensitive material, thereby increasing the free electron concentration on the surface of the gas-sensitive material and thinning the electron depletion layer, thereby causing the resistance of the material to change, thereby improving the sensitivity to formaldehyde gas.
[0007] Optionally, in step S1, the molar ratio of indium ions in the indium salt to aluminum ions in the aluminum salt is 1:0.02-0.05.
[0008] Specifically, in step S1, the molar ratio of indium ions in the indium salt to aluminum ions in the aluminum salt can be 1:0.02, 1:0.025, 1:0.028, 1:0.03, 1:0.035, 1:0.04, 1:0.05, and any ratio within the above range is acceptable. By controlling the molar ratio of indium ions in the indium salt to aluminum ions in the aluminum salt and thus controlling the amount of indium salt and aluminum salt, the prepared gas-sensitive material has higher selectivity and response speed to formaldehyde gas.
[0009] Optionally, in step S1, the weight ratio of indium salt, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.3-0.6:2-4:15-25:50-80.
[0010] Optionally, in step S1, the indium salt is indium nitrate pentahydrate or indium chloride tetrahydrate, and the aluminum salt is aluminum nitrate hexahydrate or aluminum chloride hexahydrate.
[0011] Optionally, the molar ratio of the silver ions in the silver nitrate in step S2 to the indium ions in the indium salt in step S1 is 0.05-0.08:1.
[0012] Specifically, in step S2, the molar ratio of indium ions in the indium salt to silver ions in silver nitrate can be 1:0.05, 1:0.065, 1:0.068, 1:0.07, 1:0.075, 1:0.08, or any ratio within the above range. By controlling the molar ratio of indium ions in the indium salt to silver ions in silver nitrate, the amount of Ag nanoparticles incorporated in the gas-sensitive material is controlled, so that the prepared gas-sensitive material has a balance between faster response speed and better gas selectivity, thereby enabling it to be widely used.
[0013] Optionally, in step S2, the weight ratio of citric acid, silver nitrate and NaBH4 is 1-2:1-2:1.
[0014] By adopting the above technical scheme, citric acid and NaBH4 are used as reducing agents to reduce silver ions into silver nanoparticles. In this process, citric acid not only acts as a reducing agent, but also can be wrapped on the surface of silver nanoparticles through its stable structure to play the role of a stabilizer to prevent particle aggregation, thereby obtaining highly monodisperse silver nanoparticles. NaBH4 is also a powerful reducing agent. Through the dual reducing agent system, silver nanoparticles with high purity and high dispersion are obtained.
[0015] Optionally, in step S3, the copolymerization reaction specifically includes: controlling the reaction temperature to 0-5°C, adding 5-10wt% aniline monomer solution to the dispersion of aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles obtained in step S2, ultrasonically dispersing for 5-10 minutes, adding ammonium persulfate, and stirring the reaction for 12-18 hours; wherein the molar ratio of aniline to the metal indium ions in the indium salt is 0.01-0.03:1; and the amount of ammonium persulfate used is 5wt% of the amount of aniline monomer used.
[0016] By adopting the above technical scheme, low-temperature in-situ polymerization of polyaniline is carried out on the surface of aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles, so that the polyaniline layer on the surface of the gas-sensitive material has better uniformity and higher porosity, thereby making it have a higher specific surface area. A higher specific surface area is beneficial to improving the gas-sensitive performance of the gas-sensitive material; in addition, as a conductive polymer, polyaniline has a higher specific surface area and is also beneficial to accelerating the gas-sensitive reaction and the electron transfer between the In2O3 matrix material to improve the gas-sensitive characteristics of the sensor.
[0017] Optionally, the indium oxide-based gas-sensitive material is an indium oxide-based nanorod, and the diameter of the indium oxide-based nanorod is 10-30 nm.
[0018] In a second aspect, the present application provides an indium oxide-based gas-sensitive material prepared by the above-mentioned method for preparing the indium oxide-based gas-sensitive material.
[0019] In a third aspect, the present application provides an application of an indium oxide-based gas-sensitive material prepared by the above-mentioned method for preparing an indium oxide-based gas-sensitive material in detecting formaldehyde gas.
[0020] In summary, the present invention includes at least one of the following beneficial technical effects: 1. In the present application, by preparing aluminum oxide composite indium oxide-based nanorods and sequentially doping Ag nanoparticles on their surfaces and coating them with polyaniline, the indium oxide-based gas-sensitive material obtained has high sensitivity and good selectivity to formaldehyde gas.
[0021] 2. The indium oxide-based gas-sensitive material in this application has a simple production process, easy-to-meet production conditions, and lower raw material costs than similar gas-sensitive materials, making it suitable for widespread promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a SEM image of the indium oxide-based gas-sensitive material prepared in Example 1 of the present application; Figure 2 The gas-sensitive response sensitivity test diagram of the gas-sensitive elements prepared in Application Example 1, Application Example 2 and Application Example 3 of the present application to 100 ppm formaldehyde gas at different temperatures; Figure 3The gas-sensitive response sensitivity test diagram of the gas-sensitive elements prepared in Application Example 1 and Comparative Example 1 to 100 ppm of different types of gases at 220° C.; Figure 4 This is a long-term stability test curve of the formaldehyde gas sensor prepared in Application Example 1, Application Comparative Example 1 and Application Comparative Example 2 of the present application, testing 2ppm of formaldehyde gas. DETAILED DESCRIPTION
[0023] The present application proposes a method for preparing an indium oxide-based gas-sensitive material, comprising the following steps: S1. Add indium salt, aluminum salt, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction container, mix, stir, heat to 180-210° C., react for 24-36 hours, cool to room temperature, wash and centrifuge the precipitate, and dry to obtain a precursor powder; S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 into deionized water, mixing, stirring, dropping NaBH4 solution, ultrasonically dispersing to obtain a suspension, filtering, washing the filter residue, drying, and calcining at a high temperature of 500-650° C. for 2-4 h to obtain aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles; S3. Add the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods obtained in step S2 into deionized water, add aniline monomer, disperse by ultrasonication, cause copolymerization, react for 12-18 hours, filter, wash the filter residue, and dry to obtain an indium oxide-based gas-sensitive material.
[0024] The indium oxide-based gas-sensitive material of the present application can be used in the field of formaldehyde gas detection.
[0025] The technical problem solved by the present application is that the gas-sensitive materials in the existing gas sensors are easily poisoned, and the manufacturing process is complicated, the manufacturing conditions are harsh and cannot be mass-produced. The present application prepares aluminum oxide composite indium oxide-based nanorods and sequentially dopes Ag nanoparticles on the surface thereof, and uses polyaniline for coating. The obtained indium oxide-based gas-sensitive material has high sensitivity and good selectivity to formaldehyde gas. At the same time, the manufacturing process is simple and the manufacturing conditions are easy to meet.
[0026] The present application is further described in detail below in conjunction with specific embodiments.
[0027] Example 1 The method for preparing the indium oxide-based gas-sensitive material in Example 1 comprises the following steps: S1. Add indium nitrate pentahydrate, aluminum nitrate hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction vessel, mix, stir, heat to 200°C for 30 hours, cool to room temperature, wash the precipitate, centrifuge, and dry at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium nitrate pentahydrate to aluminum ions in aluminum nitrate hexahydrate is 1:0.04. The weight ratio of indium nitrate pentahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.5:2.5:22:60.
[0028] S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 to deionized water, stirring for 10 minutes, dropping NaBH4, ultrasonically dispersing for 20 minutes, obtaining a suspension, filtering, washing the filter residue alternately with water and ethanol, drying at 80°C for 3 hours, and then calcining at 600°C for 3 hours to obtain alumina composite indium oxide-based nanorods doped with Ag nanoparticles. The molar ratio of indium ions in indium nitrate pentahydrate to silver ions in silver nitrate is 1:0.06. The weight ratio of citric acid, silver nitrate, NaBH4 and deionized water is 1.5:1.5:1:12.
[0029] S3, controlling the reaction temperature to 5°C, dispersing the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods prepared in step S2 in a weight ratio of 1:15 into deionized water, adding 5wt% aniline monomer solution, ultrasonically dispersing for 10 minutes, adding ammonium persulfate, stirring and reacting for 18 hours, filtering, washing the filter residue alternately with water and anhydrous ethanol, and drying at 60°C for 6 hours to obtain an indium oxide-based gas-sensitive material. Wherein, the molar ratio of aniline to indium ions in indium nitrate pentahydrate is 0.02:1, and the amount of ammonium persulfate is 5wt% of the amount of aniline monomer.
[0030] Example 2 The method for preparing the indium oxide-based gas-sensitive material in Example 2 comprises the following steps: S1. Add indium chloride tetrahydrate, aluminum chloride hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction vessel, mix, stir, heat to 180°C for 36 hours, cool to room temperature, wash the precipitate, centrifuge, and dry at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium chloride tetrahydrate to aluminum ions in aluminum chloride hexahydrate is 1:0.02. The weight ratio of indium chloride tetrahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.6:2:15:50.
[0031] S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 to deionized water, stirring for 10 minutes, adding NaBH4 dropwise, ultrasonically dispersing for 20 minutes, obtaining a suspension, filtering, washing the filter residue alternately with water and ethanol, drying at 80°C for 3 hours, and then calcining at 600°C for 3 hours to obtain alumina composite indium oxide-based nanorods doped with Ag nanoparticles. The molar ratio of indium ions in indium chloride tetrahydrate to silver ions in silver nitrate is 1:0.05. The weight ratio of citric acid, silver nitrate, NaBH4 and deionized water is 1.5:1.5:1:12.
[0032] S3, controlling the reaction temperature to 5°C, dispersing the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods prepared in step S2 in a weight ratio of 1:15 into deionized water, adding 5wt% aniline monomer solution, ultrasonically dispersing for 10min, adding ammonium persulfate, stirring and reacting for 18h, filtering, washing the filter residue alternately with water and anhydrous ethanol, and drying at 60°C for 6h to obtain an indium oxide-based gas-sensitive material. Wherein, the molar ratio of aniline to indium ions in indium chloride tetrahydrate is 0.01:1, and the amount of ammonium persulfate is 5wt% of the amount of aniline monomer.
[0033] Example 3 The method for preparing the indium oxide-based gas-sensitive material in Example 3 comprises the following steps: S1. Add indium nitrate pentahydrate, aluminum nitrate hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction vessel, mix, stir, heat to 210°C for 24 hours, cool to room temperature, wash the precipitate, centrifuge, and dry at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium nitrate pentahydrate to aluminum ions in aluminum nitrate hexahydrate is 1:0.05. The weight ratio of indium nitrate pentahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.6:4:25:80.
[0034] S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 to deionized water, stirring for 10 minutes, adding NaBH4 dropwise, ultrasonically dispersing for 20 minutes, obtaining a suspension, filtering, washing the filter residue alternately with water and ethanol, drying at 80°C for 3 hours, and then calcining at 600°C for 3 hours to obtain alumina composite indium oxide-based nanorods doped with Ag nanoparticles. The molar ratio of indium ions in indium nitrate pentahydrate to silver ions in silver nitrate is 1:0.08. The weight ratio of citric acid, silver nitrate, NaBH4 and deionized water is 1.5:1.5:1:12.
[0035] S3, controlling the reaction temperature to 5°C, dispersing the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods prepared in step S2 in a weight ratio of 1:15 into deionized water, adding 5wt% aniline monomer solution, ultrasonically dispersing for 10min, adding ammonium persulfate, stirring and reacting for 18h, filtering, washing the filter residue alternately with water and anhydrous ethanol, and drying at 60°C for 6h to obtain an indium oxide-based gas-sensitive material. Wherein, the molar ratio of aniline to indium ions in indium nitrate pentahydrate is 0.03:1, and the amount of ammonium persulfate is 5wt% of the amount of aniline monomer.
[0036] Comparative Example 1 Comparative Example 1 is based on Example 1, except that: in step S1 of Comparative Example 1, aluminum salt is not used for doping when preparing indium oxide nanorods. That is, step S1 is changed to: Indium chloride tetrahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water were added to a reaction vessel, mixed, stirred, heated to 180°C for reaction for 36 hours, cooled to room temperature, washed the precipitate, centrifuged, and dried at 80°C for 6 hours to obtain a precursor powder. The weight ratio of indium chloride tetrahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water was 0.6:2:15:50.
[0037] Comparative Example 2 Comparative Example 2 is based on Example 1, except that magnesium salt is used for doping when preparing indium oxide nanorods in step S1 of Comparative Example 2. That is, step S1 is changed to: Indium nitrate pentahydrate, magnesium nitrate hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water are added to a reaction container, mixed, stirred, heated to 200°C for reaction for 30 hours, cooled to room temperature, washed the precipitate, centrifuged, and dried at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium nitrate pentahydrate to magnesium ions in magnesium nitrate hexahydrate is 1:0.04. The weight ratio of indium nitrate pentahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.5:2.5:22:60.
[0038] Comparative Example 3 Comparative Example 3 is based on Example 1, except that the indium oxide-based gas-sensitive material prepared in Comparative Example 3 is not doped with silver nanoparticles, and the preparation method of the indium oxide-based gas-sensitive material in Comparative Example 3 comprises the following steps: S1. Add indium nitrate pentahydrate, aluminum nitrate hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction vessel, mix, stir, heat to 200°C for 30 hours, cool to room temperature, wash the precipitate, centrifuge, and dry at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium nitrate pentahydrate to aluminum ions in aluminum nitrate hexahydrate is 1:0.04. The weight ratio of indium nitrate pentahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.5:2.5:22:60.
[0039] S2. calcining the precursor powder obtained in step S1 at 600° C. for 3 h to obtain aluminum oxide composite indium oxide-based nanorods.
[0040] S3, controlling the reaction temperature to 5°C, dispersing the aluminum oxide composite indium oxide-based nanorods prepared in step S2 into deionized water at a weight ratio of 1:15, adding 5wt% aniline monomer solution, ultrasonically dispersing for 10 minutes, adding ammonium persulfate, stirring and reacting for 18 hours, filtering, washing the filter residue alternately with water and anhydrous ethanol, and drying at 60°C for 6 hours to obtain an indium oxide-based gas-sensitive material. Wherein, the molar ratio of aniline to indium ions in indium nitrate pentahydrate is 0.02:1, and the amount of ammonium persulfate is 5wt% of the amount of aniline monomer.
[0041] Comparative Example 4 Comparative Example 4 is based on Example 1, except that the amount of silver nanoparticles doped with the indium oxide-based gas-sensitive material prepared in Comparative Example 4 is increased, and step S2 in Comparative Example 4 is changed to: S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 to deionized water, stirring for 10 minutes, adding NaBH4 dropwise, ultrasonically dispersing for 20 minutes, obtaining a suspension, filtering, washing the filter residue alternately with water and ethanol, drying at 80°C for 3 hours, and then calcining at 600°C for 3 hours to obtain alumina composite indium oxide-based nanorods doped with Ag nanoparticles. The molar ratio of indium ions in indium nitrate pentahydrate to silver ions in silver nitrate is 1:0.12. The weight ratio of citric acid, silver nitrate, NaBH4 and deionized water is 1.5:1.5:1:12.
[0042] Comparative Example 5 Comparative Example 5 is based on Example 1, except that: in the preparation of the indium oxide-based gas-sensitive material in Comparative Example 4, polyaniline is not used to coat the aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles, that is, the preparation method of the indium oxide-based gas-sensitive material in Comparative Example 5 includes the following steps: S1. Add indium nitrate pentahydrate, aluminum nitrate hexahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction vessel, mix, stir, heat to 200°C for 30 hours, cool to room temperature, wash the precipitate, centrifuge, and dry at 80°C for 6 hours to obtain a precursor powder. The molar ratio of indium ions in indium nitrate pentahydrate to aluminum ions in aluminum nitrate hexahydrate is 1:0.04. The weight ratio of indium nitrate pentahydrate, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.5:2.5:22:60.
[0043] S2. Add citric acid, silver nitrate and the precursor powder obtained in step S1 to deionized water, stir for 10 minutes, add NaBH4 dropwise, ultrasonically disperse for 20 minutes to obtain a suspension, filter, wash the filter residue alternately with water and ethanol, dry at 80°C for 3 hours, and then calcine at 600°C for 3 hours to obtain an indium oxide-based gas-sensitive material (aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles). The molar ratio of indium ions in indium nitrate pentahydrate to silver ions in silver nitrate is 1:0.06. The weight ratio of citric acid, silver nitrate, NaBH4 and deionized water is 1.5:1.5:1:12.
[0044] Application Examples 1-3 and Comparative Application Examples 1-5 The indium oxide-based gas-sensitive materials prepared in Examples 1-3 and Comparative Examples 1-5 were used as sensing layers to prepare formaldehyde gas-sensitive elements, respectively, to obtain Application Examples 1-3 and Application Comparative Examples 1-5. The specific corresponding relationships are shown in Table 1.
[0045] Table 1 Example Application Examples Example 1 Application Example 1 Example 2 Application Example 2 Example 3 Application Example 3 Comparative Example 1 Application Comparative Example 1 Comparative Example 2 Application Comparative Example 2 Comparative Example 3 Application Comparative Example 3 Comparative Example 4 Application Comparative Example 4 Comparative Example 5 Application Comparative Example 5 The preparation methods of application examples 1-3 and comparative application examples 1-5 include the following steps: 1) Mix the above-mentioned indium oxide-based gas-sensitive material with anhydrous ethanol to form a thin paste, and place it in an ultrasonic disperser for intermittent ultrasonic dispersion for 20 minutes to reduce the agglomeration of nano-tin dioxide particles; 2) Add the uniform thin paste-like gas-sensitive material to the Al2O3 ceramic tube with electrode leads at both ends, and blow dry the ceramic tube with a hair dryer while rotating it to make the gas-sensitive material evenly coated on the surface of the ceramic tube. After drying, the thickness of the gas-sensitive material layer is about 0.2 mm; 3) The gas sensor obtained in step 2) is annealed at 500° C. for 2 h, and then assembled with a heating wire, and the electrodes are welded and aged to obtain a gas sensor.
[0046] Performance Testing 1. Take a SEM picture of the indium oxide-based gas-sensitive material prepared in Example 1. Figure 1 The microscopic morphology is nanorod-like, and the particle size is about 26nm and the specific surface area is about 72m3 / g.
[0047] 2. Measure the gas sensitivity of the gas sensor prepared in Application Examples 1-3 to 100 ppm formaldehyde gas at different temperatures. The measurement results are shown in Figure 2 .
[0048] right Figure 2 Data analysis shows that the gas-sensitive elements prepared in Application Examples 1-3 exhibit the best response value at 220°C, that is, the best operating temperature of the indium oxide-based gas-sensitive material prepared in this application is about 220°C.
[0049] 3. The selectivity of the gas sensors prepared in Application Example 1 and Comparative Example 1 to 100 ppm formaldehyde gas at 220°C was measured. The response values to five gases, formaldehyde, acetone, ethanol, triethylamine and xylene, were measured respectively. The results are shown in Figure 3 .
[0050] from Figure 3 The measurement results show that, at the same test temperature, among formaldehyde, acetone, ethanol, triethylamine and xylene test gases, the response value of the gas sensor prepared in Application Example 1 to formaldehyde is significantly higher than that of other gases, showing good formaldehyde gas selectivity.
[0051] 4. The sensitivity response values of the gas sensors prepared in Application Examples 1-3 and Comparative Application Examples 1-5 to 0.2 ppm, 2 ppm and 50 ppm formaldehyde gas were measured respectively. The measurement results are shown in Table 2.
[0052] Table 2 By analyzing the data in Table 2, it can be found that the sensitivity response values of Application Examples 1-3 to formaldehyde gas of different concentrations are significantly better than those of Application Comparison Examples 1-5. Therefore, the indium oxide-based gas-sensitive material prepared in the present application has high sensitivity and good selectivity to formaldehyde gas, and the production process is simple and the production conditions are easy to meet.
[0053] 1. The gas sensors prepared in Application Example 1, Application Comparative Example 1 and Application Comparative Example 2 were used to measure the sensitivity response value of 2 ppm formaldehyde gas at 15, 30, 60, 90, 120, 150 and 180 days respectively. The test results are shown in Figure 4 .
[0054] Through Figure 4Analysis shows that the sensitivity response value of the gas-sensitive element prepared in Application Example 1 decreases significantly less over time than those in Application Comparison Example 1 and Application Comparison Example 2. This shows that the use of aluminum salts for doping in the preparation of indium oxide nanorods plays an important role in maintaining the long-term stability of the gas-sensitive material. The indium oxide-based gas-sensitive material prepared in the present application has good long-term stability, and even after 180 days, the decrease in its sensitivity response value is still small.
[0055] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing an indium oxide-based gas-sensitive material, characterized in that: The following steps are involved: S1. Add indium salt, aluminum salt, polyvinyl pyrrolidone, polyethylene glycol and deionized water into a reaction container, mix, stir, heat to 180-210° C., react for 24-36 hours, cool to room temperature, wash and centrifuge the precipitate, and dry to obtain a precursor powder; S2, adding citric acid, silver nitrate and the precursor powder obtained in step S1 into deionized water, mixing, stirring, dropping NaBH4 solution, ultrasonically dispersing to obtain a suspension, filtering, washing the filter residue, drying, and calcining at a high temperature of 500-650° C. for 2-4 h to obtain aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles; S3. Add the Ag nanoparticle-doped aluminum oxide composite indium oxide-based nanorods obtained in step S2 into deionized water, add aniline monomer, disperse by ultrasonication, cause copolymerization, react for 12-18 hours, filter, wash the filter residue, and dry to obtain an indium oxide-based gas-sensitive material.
2. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: In the step S1, the molar ratio of indium ions in the indium salt to aluminum ions in the aluminum salt is 1:0.02-0.
05.
3. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: In the step S1, the weight ratio of indium salt, polyvinyl pyrrolidone, polyethylene glycol and deionized water is 0.3-0.6:2-4:15-25:50-80.
4. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: In the step S1, the indium salt is indium nitrate pentahydrate or indium chloride tetrahydrate, and the aluminum salt is aluminum nitrate hexahydrate or aluminum chloride hexahydrate.
5. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: The molar ratio of the silver ions in the silver nitrate in step S2 to the indium ions in the indium salt in step S1 is 0.05-0.08:
1.
6. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: In step S2, the weight ratio of citric acid, silver nitrate and NaBH4 is 1-2:1-2:
1.
7. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: In the step S3, the copolymerization reaction specifically includes: controlling the reaction temperature to 0-5°C, adding 5-10wt% aniline monomer solution to the dispersion of the aluminum oxide composite indium oxide-based nanorods doped with Ag nanoparticles obtained in step S2, ultrasonically dispersing for 5-10 minutes, adding ammonium persulfate, and stirring the reaction for 12-18 hours; wherein the molar ratio of aniline to indium ions of the indium salt in the step S1 is 0.01-0.03:1; and the amount of ammonium persulfate used is 5wt% of the amount of aniline monomer used.
8. The method for preparing an indium oxide-based gas-sensitive material according to claim 1, characterized in that: The indium oxide-based gas-sensitive material is an indium oxide-based nanorod, and the diameter of the indium oxide-based nanorod is 10-30 nm.
9. An indium oxide-based gas-sensitive material prepared by the method for preparing an indium oxide-based gas-sensitive material according to any one of claims 1 to 7.
10. Use of the indium oxide-based gas-sensitive material prepared by the method for preparing the indium oxide-based gas-sensitive material according to any one of claims 1 to 7 in detecting formaldehyde gas.
Citation Information
Patent Citations
Formaldehyde gas sensitive device with laminated sensitive layer and preparation method thereof